Open Access Article
Leonard
Kwati
*acd,
Kuninori
Miyazaki
b,
Christian
Dellen
c,
Mariya E.
Ivanova
c,
Wendelin
Deibert
c,
Julia
Wolter
c,
Wilhelm A.
Meulenberg
c,
Olivier
Guillon
c,
Veeramani
Vediyappan
d,
Tatsumi
Ishihara
ad and
Hiroshige
Matsumoto
ad
aCenter for Energy Systems Design (CESD), International Institute for Carbon Neutral Energy Research (WPI-I2CNER), Kyushu University, 744 Motooka, Nishiku, Fukuoka 819-0395, Japan. E-mail: kwati@i2cner.kyushu-u.a.jp; Tel: +81-092-802-6706
bStrategic Institute of Technology and Research Center, 992-1 Nishioki, Himeji, Hyogo 671-1292, Japan
cInstitute of Energy Materials and Devices (IMD) Materials Synthesis and Processing (IMD-2), Forschungszentrum Jülich GmbH, Wilhelm-Johnen-Straße 52428, Germany
dInternational Institute for Carbon Neutral Energy Research (WPI-I2CNER), Kyushu University, 744 Motooka, Nishiku, Fukuoka 819-0395, Japan
First published on 9th April 2025
Ceramic proton-conducting electrolytes are highly appealing for large-scale hydrogen production via steam electrolysis at low to moderate temperatures. However, processing such electrolytes for industrial purposes poses several challenges. Our research demonstrates an effective tape-casting route that produces flat, planar BaZr0.44Ce0.36Y0.2O3−δ protonic half-cells with impressive dimensions of up to 50 mm × 50 mm. The cells are constructed using NiO-SrZr0.5Ce0.4Y0.1O3−δ as the fuel electrode, which ensures minimal warping and no cracks in the end-fired state. The electrolyte is dense and gas-tight after co-firing at 1300 °C and achieves a He leakage rate well within the threshold necessary for cell operation (∼5 × 10−5 hPa dm3 s−1 cm2)−1. Using B0.5La0.5CoO3−δ as the steam electrode, the cell achieves an electrolysis voltage of 1.3 V at a current density of 1.37 A cm−2 at 600 °C. Moreover, they also exhibit high durability, lasting over 1000 hours of continuous hydrogen generation with no observable degradation, which is a testament to their reliability. In addition, scanning electron microscopy paired with energy-dispersive X-ray spectroscopy, Raman spectroscopy, and X-ray diffraction were employed to examine the structural changes in the half-cells after sintering at different temperatures. It is apparent from the latter techniques that upon sintering above 1350 °C, the electrolyte undergoes evident structural changes with new defects that affect the perovskite host. Finally, our work paves the way for the cost-effective fabrication of planar proton-conducting electrolysis cells.
Solid oxide steam electrolysis (SOECs) at moderate temperatures (300–600 °C) offers excellent prospects for efficient and cost-effective large-scale hydrogen production,4,5 depending on the source of the electricity used. This temperature domain also allows seamless heat integration options and non-noble materials, which will benefit cost. Furthermore, the overpotential is lower, as the electrolysis reactions are favored by kinetics at higher temperatures. It is also worth noting that SOECs can operate in reverse mode as fuel cells, enabling the conversion of hydrogen back into electricity. This sets them apart from alkaline and PEM electrolysis, allowing them to provide grid-balancing services when paired with hydrogen storage facilities.1,4,6
Proton-conducting ceramic (PCC) solid-oxide represents viable, moderate-temperature electrolytes for these devices, given their high ionic conductivity and inherent advantages in the gas flow configuration over traditional solid oxide cells in which the electrolyte is an oxygen ion conductor.7–11 Protonic conductivity in this class of materials relies on the partial filling of vacant oxygen sites by water to yield mobile proton interstitials bound to lattice oxide ions. The inserted protons subsequently exhibit relatively high mobility and give rise to the significant protonic conductivity observed.11,12 State-of-the-art protonic electrolytes comprise acceptor-doped perovskite oxides within the Ba(ZrxCe1−x)YyO3−δ solid solution series.9 Compositions such as BaZr0.4Ce0.4Y0.1Yb0.1O3−δ (BZCYYb411)8 BaCe0.55Zr0.3Y0.15O3−δ (BCZY3), BaZr0.1Ce0.7Y0.2O3−δ (BZCY172),13 and BaZr0.1Ce0.7Y0.1Yb0.1O3−δ (BZCYYb1711)14,15 are among the most reported within this series. In addition, recent progress in developing suitable air electrode materials explicitly tailored for these electrolytes16 has made it possible to achieve high-performing proton conducting fuel cells (PCFC),8,10,17 substantially lower cell voltages at higher current densities, and high current efficiencies in protonic ceramic electrolysis cells (PCEC).18,19 However, to date, most reported cells have been realized mainly with laboratory-scale button cells having a relatively limited cell size (less than 3 cm2) and electrode surface area (0.2–0.5 cm2). Only a few systematic investigations have focused on scale-up efforts.20,21 This is due to the challenges of scaling up proton-conducting ceramic solid oxide.22 Besides the desirable high current densities of the small-size button cells, in many instances exceeding (in magnitude) 1.0 A cm−2 even at 600 °C under a thermo-neutral operating voltage of ∼1.3 V, concurrent hydrogen generation rates are scarce, let alone over several continuous hours of operation with only a few exceptions.23 Long-term durability lasting hundreds of hours with simultaneous successive hydrogen generation is greatly needed to advance PCEC technology.14
As a technical issue, these electrolyte types generally require high sintering temperatures (≥1500 °C) and a longer duration to densify completely. Such high temperatures can increase the overall processing cost in the fabrication process and cause the evaporation of essential elements like barium, leading to off-stoichiometry and decreasing ionic conductivity, which is unfriendly to the device's performance.7 Recent studies have also shown that the sintering temperature of such electrolytes in bilayer structures can be reduced when in contact with a NiO-containing electrode, as NiO acts as an inherent sintering aid.8–10 To attain the desired microstructures in such a bilayer consisting of a porous electrode and dense electrolyte, the sintering schedule must be carefully designed, considering the shrinkage of both layers. Moreover, similar to SOEC technology, there are significant challenges in scaling up flat, robust, and durable proton conducting electrochemical cells (PCECs). These devices are complex multilayer structures with varying compositions and microarchitectures, making them susceptible to warping during sintering. This warping behavior often leads to poor sealing and imposes additional mechanical stress on the cells during operation. Notably, the degree of warping tends to increase with larger cell sizes. Therefore, the cells’ size and flatness are critical factors in the design of PCEC stacks, which are essential for commercial hydrogen production applications. Thus, careful control over chemical incompatibilities between the cell components20 is necessary to avoid cracked, pinhole defects, and performance loss.
This study demonstrates a cost-effective tape casting and screen-printing route to fabricate flat planar cathode-supported PCEC cells with NiO-SrZr0.5Ce0.4Y0.1O3−δ (NiO-SZCY541) as the negative electrode. By carefully controlling powder properties and slurry formulations, BaZr0.44Ce0.36Y0.2O3−δ (BZCY44362) half-cells of dimensions up to 50 mm × 50 mm × 0.5 mm with diminished warping and no cracks in the end-fired state have been fabricated. Minimal strontium segregation from the NiO-SZCY541 electrode during sintering significantly influences the electrolyte densification and potentially mitigates the half-cell warped behavior. Furthermore, scanning electron microscopy in combination with energy-dispersive X-ray spectroscopy, Raman spectroscopy, and X-ray diffraction were used to analyze the structural modifications of the half-cells upon sintering at varying temperatures. It is apparent from the latter techniques that upon sintering above 1350 °C, the electrolyte undergoes evident structural changes with new defects that affect the perovskite host.
:
1 ratio, with 0.4 wt% methyl ethyl ketone added to improve the viscosity. Raman spectroscopy mappings were taken using a Renishaw inVia Qontor confocal Raman microscope. The system was used to gather Raman mappings of the sample surfaces and polished cross-section samples. All the Raman measurements were conducted with a green laser (532 nm wavelength) and a 2400 l mm−1 grating.
:
40) dispersed in an ethanol and methyl ethyl ketone (66
:
34%) mixture together with Nuosperse FX9086 (1%) (Elementis Specialties, Inc., London, UK) as the dispersing agent. Furthermore, polyvinyl butyral (Butvar PVB-98 (4.66%), Solutia Inc., St. Louis, MO, USA) and Solusolv 2075 (Solutia Inc., St. Louis, MO, USA) were added as plasticizers, along with polyethyleneglycol PEG 400 (Merck Schuchardt, Hohenbrunn, Germany) serving as a binder (2.33%). The mixture was homogenized in a Thinky vacuum mixer and left to rest for 48 hours to de-air and completely dissolve the binder before casting. The electrolyte slurry was prepared using a previously reported two-step procedure with minor modifications and cast onto a silicone-coated polymeric (polyethylene terephthalate) foil.2,3 After proper drying at room temperature, a functional NiO-SZCY541 layer (without pore former) was cast directly on top of the electrolyte layer, followed by the support NiO-SZCY541 (with 5 wt% rice starch as pore former) slurry with a six-hour drying interval. This approach guarantees the formation of defect-free electrolyte layers, thanks to the superior surface quality of the foil. The green tapes were then precisely cut to the desired dimensions and sintered at 1300 °C, 1350 °C, and 1400 °C for 5 and 10 hours, respectively. Half-cells measuring 50 × 50 mm2 and 22 mm diameter with the following configurations BZCY44362|NiO-BZCY44362 (dense layer) |NiO-BZCY44362 (porous)| and BZCY44362|NiO-SZCY541 (dense layer)|NiO-SZCY541 (porous)| were used for characterisation. While flat half-cells of 50 × 50 mm2 and 22 mm in diameter could be easily produced for the latter configuration, the former could only yield flat half-cells with a diameter of 22 mm. The thickness of the electrolyte was controlled by adjusting the gap between the polymer foil and the doctor blade. The curvature of the half-cells after sintering was measured using a white light topography unit (CT 350, CyberTechnologies, Ingolstadt, Germany). Thermo-gravimetric analysis (TGA) and differential thermal analysis (DTA) coupled with mass spectrometry (MS) were carried out using a Netzsch S.T.A. 409C system to understand the decomposition behavior of the organic additives in both the electrolyte and NiO-based substrate single layers. Measurements were conducted at a maximum temperature of 1000 °C using a heating rate of 5 °C min−1 and in a constant flow of nitrogen and oxygen gases at ambient pressure. The warpage/bending behavior of the half-cell was investigated by comparing their shrinkage behavior using a TOMMI plus optical dilatometer (Fraunhofer I.S.C., Würzburg, Germany). The instrument features a furnace with quartz windows, a light source, and a camera. It continuously records images of the sample silhouette during heat treatment, enabling precise determination of shrinkage through careful selection of the sample geometry. To further improve the mechanical properties of the half-cells, the co-cast layers were further compressed by applying a pressure of 8 MPa at 80 °C using a warm press by P/O Weber. The gas tightness of the 50 × 50 mm2 half-cell was evaluated using helium leakage rate measurements. A mass spectrometer measured gas flow through the half-cell at a pressure difference of 1000 hPa, which was then normalized for an area of 16 cm2 and a pressure difference of 100 hPa. Finally, a Ba0.5La0.5CoO3−δ anode slurry was prepared by mixing the powder with terpineol (containing 5 wt% ethylcellulose). This mixture was screen-printed onto the electrolyte surface with an active area of 0.5 (22 mm diameter half-cell) and 1 cm2 (50 × 50 mm2 half-cell), achieving a final thickness of ∼30 μm after sintering at 800 °C for 1 hour.
min−1) carrier gas. Simultaneously, the cathode was supplied with 1% H2/Ar 99% (50 mL min−1), maintaining a water vapor pressure of PH2O = 1.9 × 103 Pa. A hygrometer chilled mirror (UHQ-4P, Buck Research Instruments LLC, Tokyo, Japan) monitored the anode inlet's water vapor pressure. Gas lines were heated at 120 °C to prevent the condensation of water vapor. Hydrogen evolution was determined by measuring the increase in hydrogen concentration in the cathode gas outlet by gas chromatography (Varian CP-4900 micro-Gas Chromatograph equipped with a micro-machined Thermal Conductivity Detector (TCD), Agilent Technologies Inc., Tokyo, Japan). Faradaic efficiencies were obtained based on the experimentally measured and theoretical hydrogen generation rates at fixed current densities using the following formula.
485 C mol−1), and J is the applied current density in (A). Energy efficiency was calculated based on the lower heating value of hydrogen, as shown in the equation below.
kJ
mol−1 and V is the corresponding voltage (V). The electrochemical performance of single cells was evaluated using a potentiostat (Bio-Logic, VMP-250) at operating temperatures from 450 to 600 °C. Impedance spectra were measured under open circuit voltage (OCV) in the frequency range from 1 MHz to 0.1 Hz with an AC amplitude of 10 mV. Humidified H2 (5% H2O) and air with flow rates of 250 mL m−1 were introduced at the cathode and anode of the 50 mm × 50 mm cell, respectively.
4 at the perovskite B-site.9,11 As a result, the unique composition BaZr0.44Ce0.36Y0.2O3−δ (BZCY44362) exhibits a high conductivity (10.1 mS
cm−1 at 500
°C in wet 1% H2), excellent chemical stability under steam and CO2, as well as satisfactory processability.9 This target composition with modified versions and a composite NiO-SZCY541 were chosen for the half-cell fabrication via an inverse tape casting approach.20 Choosing a suitable starting powder is crucial to ceramic processing, as it significantly influences the quality of the tapes and their sintering properties. The BZCY44362 electrolyte and SZCY541 powder properties used were thus first ensured via a two-step calcination process at 900 and 1200 °C, respectively, with subsequent milling (in ethanol).
![]() | ||
| Fig. 1 (a) Schematic illustration of a steam proton conducting electrolysis cell (PCEC). (b) BZCY44362-based cell in the end-fired state with the microstructure after reduction. | ||
This treatment leaves both materials with a comparably low particle size distribution d50 of 0.68 and 0.70 μm and specific surface area (Aspec) of 5.1 and 4.7 m2 g−1, respectively, which are satisfactory for making optimal slurries for tape casting and providing the necessary driving force for densification during sintering. Fig. S1 (ESI†) presents SEM images of the powders and particle size distribution used in the slurry for casting. Sequential tape casting was used to fabricate the layers, after which green tapes were cut into 65 × 65 mm2 using a scalpel blade for co-sintering to obtain an integrated electrolyte/NiO composite ceramic known as half-cell.20 Deformation and warpage of the half-cells were controlled by adequately optimizing the binder, plasticizer, and dispersant amount. The sintering process of tape-cast layers also plays a vital role in fabricating high-quality flat ceramic components. The burn-out behavior of the organic additives in the tape-cast layers has been discussed in our previous manuscripts and briefly in the subsequent section. A slow ramp rate of 1 °C min−1 was used for sintering, with holding temperatures of 300 °C and 600 °C maintained for 30 minutes. After this, a 2 °C min−1 ramp rate was employed, as shown below. Flat, 50 × 50 mm2 half-cells, after sintering, were routinely obtained by this procedure, corresponding to 23.1% shrinkage along the axes. We also noted that a cathode substrate support of 450 μm in the end-fired state was sufficient to induce mechanical strength and mitigate the overall half-cell curvature. Table S1 (ESI†) presents suitable processing parameters for the green tape fabrication. The NiO-SZCY541-based half-cells are flat and achieve a dense, gas-tight BZCY44362 electrolyte layer after co-sintering at 1300 °C for 5 hours, which is about 200 °C lower than required for the electrolyte alone. In contrast, the same electrolyte composition did not densify enough when placed on the NiO-BZCY44362 electrode substrate at 1350 °C, probably because of Ba loss and yttrium displacement from the perovskite B-site into the A-site resulting in lattice shrinkage, which probably deteriorates the electrolyte densification. The mechanism of barium evaporation deteriorating the electrolyte sintering is still not precise. Based on observation, however, the latter half-cell appeared dense after sintering at 1450 °C but showed significant edge warping in the 50 × 50 mm2 size configuration. Flat half-cells of this size could not be made using the NiO-BZCY44362 electrode substrate, so the dimensions were reduced to 22 mm in diameter with a 450 μm support thickness for cell operation and comparison. A sintering temperature of 1500 °C and a dwell time of 3 hours were thus required. This high temperature also triggers yttrium precipitation around the nickel oxide grain vicinity, which may result in a stoichiometric imbalance, as discussed in the subsequent section. This imbalance can reduce the concentration of oxygen vacancies in the material, negatively affecting the electrolyte's conductivity and, consequently, the cell's performance. For such half-cells, the structural and compositional uniformity of the cement electrode and the aligned shrinkage behaviors of the electrode and electrolyte layers are critical for a successful scale-up. Any differences in shrinkage from temperature changes can cause flaws in the support's biaxial constraints, leading to severe issues like pinholes, cracks, and delamination in the half-cells after sintering. These problems are also likely to worsen as the half-cell size increases. To further comprehend how the NiO-SZCY541 composite promotes the densification of the electrolyte, optical dilatometry was used to investigate the lateral shrinkage behavior of both the single electrolyte and bi-layers. Fig. 2(a) compares the lateral shrinkage of the single BZCY44362 layer, the NiO-BZCY44362-BZCY44362 bilayer, and the NiO-SZCY541-BZCY44362 bilayer. The NiO-SZCY541 bilayer shows a higher shrinkage of 34%, compared to 26% for the NiO-BZCY44362 half-cells. This indicates the latter bilayer should, in principle, assist and improve the sintering activity of the electrolyte layer. In comparison, the BZCY44362 single layer shrunk only by ∼10%. This is expected since the layer has less organic content and finer particle size. Fig. 2(b) and (c) also compare the surface microstructural view of the same electrolyte composition on both electrode substrates. Fig. 2(c) clearly shows that the NiO-SZCY541-based electrode significantly impacts sintering and grain growth, as indicated by the noticeable differences in grain size and relative density. In contrast, the NiO-BZCY44362-based half-cell (Fig. 2(b)) remains porous even after being sintered at 1350 °C for 5 hours. Thus, the NiO-SZCY541 electrode substrate not only facilitates sintering but also aids in densifying the electrolyte and promoting grain growth, which allows for reduced processing temperatures. Furthermore, Helium leak rate tests performed on the 50 × 50 mm2 NiO-SZCY541 base half-cell configuration after sintering at 1300 °C for 5 hours indicate an average leak rate of ∼5 × 10−5 hPa dm3 (s cm2)−1, which falls well within the acceptable range for high-quality gas-tight electrolytes used in cell operation.
Recent literature suggests that the fundamental mechanism involved in the sintering of barium-based electrolytes is through the formation of a BaY2NiO5 transient phase, which is formed at the electrode and supplied to the electrolyte during sintering to aid the process. While this is recognized, it may not be the primary mechanism in the present study.
It illustrates the elemental distributions of barium (Ba), zirconium (Zr), cerium (Ce), yttrium (Y), and nickel (Ni). The Y maps reveal prominent Y-rich regions that align with the Y2O3 phases observed in the X-ray diffraction pattern in Fig. 3(b). This observation is consistent with similar findings reported in the literature.11,20,24 In contrast, Y2O3 phases are rarely observed or utterly absent in the BZCY44362|NiO-SZCY541 half-cell sintered at 1350 °C, as shown in Fig. 3(c). Furthermore, the selected area electron diffraction (SAED) in Fig. 3(d) shows lattice fringes and prominent lattice planes attributed to orthorhombic SZCY541,24 initially present only in the substrate layer.
Moreso, EDS elemental maps of the cross-section of the latter half-cell shown in Fig. S4 (ESI†) reveal that Sr is predominantly present and uniformly distributed throughout the BZCY44362 electrolyte layer. The investigation into the precise amount of incorporated Sr is ongoing. As discussed, using the NiO-SZCY541 electrode substrate minimizes deformation and warpage, resulting in consistently flat half-cells measuring 50 mm × 50 mm. While the precise cause of this effect remains unclear and is still under investigation, post-sintering measurements taken with a white light topography unit indicate an approximate flatness of 0.2 mm, as shown in Fig. 4. It is likely that strontium diffusion from the latter substrate to the electrolyte layer compensates for some of the barium loss, which may help mitigate the deformation and warpage of the half-cells.
The minor differences can be attributed to partial hole conductivity in the electrolyte, consistent with other literature reports. Additionally, the OCVs for the larger 50 × 50 mm2 NiO-SZCY541-based cell reached 1.09 V at a temperature of 600 °C, indicating that there was also no apparent electronic or gas leakage. Fig. 5(c) depicts current–voltage (I–V) curves for the BZCY44362 (10 μm)|NiO-BZCY44362 and BZCY44362 (10 μm)||NiO-SZCY541 based cell measured at 600 °C, under a controlled supply of humidified 1% O2/99% Ar and 80% H2O to the air electrode and 1% H2/Ar 99% at the fuel electrode as the sweep gas. The cell based on BZCY44362 (∼10 μm)|NiO-BZCY44362 achieved an electrolysis current density of 1 A cm−2 at 600 °C, with an overpotential of 1.2 V. In contrast, the BZCY44362 (∼10 μm)|NiO-SZCY541 cell also achieved the same current density but with a significantly lower overpotential of only 0.59 V. The performance of the latter cell improves when an electrolyte approximately 8 μm thick is used. At temperatures of 600, 550, 500, and 450 °C, the cell produces electrolysis voltages of 1.3 V at current densities of approximately 1.37, 0.98, 0.5, and 0.22 A cm−2, respectively, Fig. 5(d) and Fig. S6 (ESI†), which are among the best-reported performances at such low temperatures for similar electrolyte composition8,10,17,25Fig. 6(d) and Table S3 (ESI†). For example, at 500 °C, Choi et al.8 showed a current density of 0.5 A cm−2 at 1.4 V, while Ding et al.17 achieved 0.84 A cm−2 and Duan et al.10 reached 0.74 A cm−2, whereas the present work achieves 0.87 A cm−2 under the same applied voltage and temperature. These results suggest the processing technique mentioned above and the efficacy of the NiO-SZCY541-mediated sintering of the electrolyte at lower temperatures are highly effective in improving the performance of PCECs and their potential operation at lower temperatures. The amount of hydrogen gas produced during the electrolysis operation was quantified by gas chromatography. The evolved hydrogen rate follows Faraday's law and is proportional to the current density, exhibiting faradaic efficiencies close to 90% (Fig. S6, ESI†) for the BZCY44362|NiO-SZCY541 based cell and 85% for the BZCY44362|NiO-BZCY44362 cell. The deviations at higher current densities are ascribed to intrinsic electronic leakage through the electrolyte, consistent with several other experimental investigations.7–9,17,25 Because of concerns about the impact of Sr segregation on the electrolyte conductivity, the behavior of the electrolyte conductivity with some amount of Sr doped in the A-site was investigated on sintered pellets. Fig. 5(e) and (f) show the ionic conductivity plot versus temperature and Sr content. As observed in Fig. 5(e), 10 mol% Sr-doped BZCY44362 exhibited nearly similar conductivity to pure BZCY44362 at 600 and 500 °C in wet air (PH2O = 1.9 × 103 Pa). However, as the Sr content in the A-site increased (Fig. 5(f)), there is a slight linear decrease in conductivity, although not significant. The electrochemical impedance spectroscopy (EIS) of the BZCY9144362 (Ba0.9Sr0.1Zr0.44Ce0.36Y0.2O3−δ) based cell was evaluated in dry air (PO2 = 0.21 atm), 20%, and 80% H2O in the steam side electrode, with a 1% H2 balance of Ar (99%) in the fuel side electrode. Increasing the steam pressure from 20% to 80% also enhances the electrode reaction, which is evidenced by the decrease in the EIS and the improvement in the IV characteristics, as shown in Fig. 5(g) and (h).
Furthermore, the long-term durability of the cell was examined at a constant current density of 0.5 A cm−2 at 600 °C, as illustrated in Fig. 6(a), with the 10 mol% Sr doped BZCY9144362 (Ba0.9Sr0.1Zr0.44Ce0.36Y0.2O3−δ), electrolyte. The cell achieved a faradaic efficiency of about 85% and maintained its performance for over 1000 hours without any noticeable degradation or changes in the microstructure Fig. 6(c). Based on the later results, the calculated amount of electricity to produce 1 Nm3 of H2 is ∼3.5 kW h within the as-measured durability range, as shown in Fig. 6(b).
Fig. 7(a) presents the line average Raman spectra for a polished cross-section of a half-cell sintered at 1300 °C/10 h, illustrating the mapped area starting in the electrolyte at the top and extending into the fuel electrode below. The transition between electrolyte and electrode is best seen in the rising Raman signal around 1100 cm−1, which reflects the NiO in the fuel electrode. The spectra are characterized by peak positions typical of BZCY perovskite-type oxides.26,27 Additionally, a well-resolved peak at ∼296 cm−1 is observed in Fig. 7(b) and Fig. S8 (ESI†), which does not appear after a dwelling time of 5 hours, even following sintering at 1350 °C (see Fig. 7(c) and Fig. S7, ESI†). The modes around 74 and 145 cm−1 are associated with A-site cation ordering/symmetry primarily attributed to deformational motions and stretching vibrations of the Ba–[(Zr/Ce/Y)]O6.28–30 Upon sintering at 1400 °C, two distinct peaks at 110 and 173 cm−1 are observed, indicating structural changes within the Ba(Zr, Ce, Y)O3 system, as shown in Fig. 7(d). These peaks are attributed to alterations in the Ba–O stretching and O–Ba–O bending modes, suggesting deviations from the electrolyte's ideal cubic symmetry (space group Pm
m). Their appearance is related to local symmetry reduction due to Ba loss during sintering (see equation below) and Sr substitution in the A-site consistent with previous literature reports.24,29,30 Furthermore, the Raman intensity of the X–O (X = Ce, Zr, Y) stretching mode around 615 cm−1 is significantly reduced and shifted, indicating a clear and definitive structural change in the material Fig. S11 (ESI†).
| BZCY44362 | BaZr0.44Ce0.36Y0.2O3−δ |
| SZCY541 | SrZr0.5Ce0.4Y0.1O3−δ |
| BLC55 | Ba0.5La0.5CoO3 |
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d5ma00028a |
| This journal is © The Royal Society of Chemistry 2025 |