We first designed the thermoresponsive star-shaped polymer with heteroarm structure based on methacrylates by living radical polymerization with Ru catalyst. The lowest critical solution temperature (LCST) of the heteroarm polymer was controlled within the range 26–52 °C by changing the initial ratio of diethylene glycol methyl ether methacrylate (DEGMA) and triethylene glycol methyl ether methacrylate (TEGMA) in the copolymerization. The synthesized heteroarm star-shaped polymer consisted of P(DEGMA-stat-TEGMA), with a unit composition of DEGMA
:
TEGMA = 83
:
17 and LCST of 35 °C, and poly(methyl methacrylate) (PMMA), and possessed approximately six arms of P(DEGMA-stat-TEGMA) and approximately two arms of PMMA. This heteroarm star-shaped polymer was insoluble in water. However, the star-shaped polymer-coated surface showed thermoresponsivity, in which the contact angle of the captive bubble changed from 131 ± 0.6° at 20 °C to 126 ± 1.9° at 40 °C. This result indicates that such heteroarm star-shaped polymers can be promising materials for constructing thermoresponsive surfaces using simple coating methods.
Thermoresponsive polymers, especially in aqueous media, have been intensively studied in the biomedical area because of their use of a safe solvent and easy application. The polymer main chain is aggregated above the cloud point temperature due to dehydration in water, although it is soluble in water because of sufficient hydration at temperatures lower than the cloud point, so there is a cold “lower critical solution temperature” (LCST). It is well known that the LCST of poly(N-isopropyl acrylamide) (PNIPAM) is 32 °C, which is very close to physiological temperatures.10 However, it is important to create novel thermoresponsive polymer materials besides PNIPAM, to develop a variety of polymer materials. For example, poly(vinyl ether),11,12 polyacrylate13 and polymethacrylate,14–16 and poly(trimethylene carbonate) derivatives17,18 bearing oligo(ethylene glycol) (OEG) units have been reported. Furthermore, poly(vinylcaprolactam),19 poly(N-vinylisobutyramide),20,21 and some other polysaccharides and polypeptides have also been investigated, and their applications studied. Once well-designed polymer main chains are produced, it is possible to use them in various polymer structures to form materials such as micelles and gels.
Star-shaped polymers are an interesting polymer structure, in which many polymer chains are attached to a central core, and they have the characteristics of branched polymers as well as spherical morphology.22,23 The multifunctional initiator method, in which branch polymers are elongated from initiators bearing many initiator groups, and the arm-first method, in which pre-made branch polymers are combined with coupling agents, are well-known methods for the synthesis of star-shaped polymers. Star-shaped polymers with hydrophobic components in the core and hydrophilic polymers in the outer shell are called unimolecular micelles, in comparison to conventional micelles that are formed by the weak physical aggregation of amphiphilic polymers. The structural stability of star-shaped polymers is expected to be useful for applications such as gene and drug delivery and removal of organic compounds from water.
The properties of star-shaped polymers with thermoresponsive moieties have been investigated. It has been reported that the LCST values can changed depending on the number of arms,24,25 so it is important to design and control the polymer structures for thermoresponsive star-shaped polymers. By evaluating thermoresponsive star-shaped polymers obtained by multifunctional initiator methods, the effect of the number of branches on the LCST and the construction of precise thermoresponsive networks using these polymers has been reported. Four-armed types, such as the simple star-shaped polymers, have been investigated using porphyrin26,27 and benzene.28 These four-arm types can be applied for gel formation as well.29,30 Various kinds of thermoresponsive polymers have been introduced into star-shaped polymers, such as NIPAM,31N-vinylcaprolactam,32 methacrylate,33 and oxazoline.34 Since the arm part is a partially linear structure, the copolymers were sometimes used as arm structures. These approaches enable various polymer materials to be created. For example, the block copolymer of NIPAM and N-methylolacrylamide was synthesized for the arm of a star-shaped polymer,35 and utilized as a drug delivery system. The block copolymers of acrylate and methacrylates with OEG groups were also prepared by atom transfer radical polymerization (ATRP) for use in producing star-shaped polymers,36 as well as anionic polymerization methods.37 Interestingly, the helical structures of the arm part were also designed as block copolymers of isocyanide.38 Unlike simple linear polymers, the star-shaped polymer possesses unique polymer structures, so it could be utilized for some applications by tuning the properties using copolymers. For example, hydrogels with thermoresponsive moieties at cross-linking points,39 cell adhesive control,40 and reduction-controlled drug delivery.41
Moreover, heteroarm star-shaped polymers or miktoarm star-shaped polymers are defined as polymers in which different types of branch polymers are introduced into the same star-shaped polymer structure. Unlike the case of using random or block copolymers as the branch polymers of star-shaped polymers, the different properties of the branch polymers cause phase separation within the star-shaped polymer, resulting in unique aggregation behavior, such as Janus particles. Lodge and co-workers reported that heteroarm star-shaped polymers consisting of three types of hydrophilic/hydrophobic/fluorinated polymer chains from hamburger-like aggregates in water can encapsulate different compounds at each aggregation site.42,43 Chen and co-workers utilized polycaprolactone as a hydrophobic arm and polymethacrylate with OEG as a hydrophilic arm to prepare a pH-responsive heteroarm star-shaped polymer.44
We have previously reported heteroarm star-shaped polymers composed of hydrophilic poly(hydroxymethyl methacrylate) (PHEMA) and hydrophobic poly(methyl methacrylate) (PMMA), using Ru catalyst living radical polymerization technique as an interfacial functional material.45 When the star-shaped polymer is coated on polyethylene terephthalate (PET) film, the star-shaped polymer is physically anchored to the surface due to hydrophobic interactions between PMMA and PET, and the PHEMA chains are considered to adopt a polymer brush-like structure swollen in water. The surface therefore exhibits a larger bubble contact angle in water than the linear PHEMA-coated surface, greatly reducing the adhesion of Escherichia coli and platelets. Therefore, by assigning roles to each branch polymer characteristic of the heteroarm, it is possible to functionalize the surface by a facile method.
Recently, several examples of thermoresponsive heteroarm star-shaped polymers have been reported. For example, Brooks, Kizhakkedathu, and co-workers reported RAFT and ATRP combination to produce thermoresponsive heteroarm star-shaped polymers with N,N-dimethylacrylamide and NIPAM.46 Furthermore, Plamper and co-workers selected the poly(ethylene oxide), poly(propylene oxide), and poly(N,N-dimethylaminoethyl methacrylate) as heteroarms for thermoresponsive star-shaped polymers.47 Recently, microflow systems have been utilized to tune the star-shaped polymer with heteroarms for methacrylate with OEG units and N,N-dimethylaminoethyl acrylate.48 Aoshima and co-workers systematically synthesized thermoresponsive heteroarm star-shaped polymers,49,50 including fluorine-containing block copolymers and heteroarm star-shaped polymers with poly(vinyl ether) backbones. However, to the best of our knowledge, there are no examples of thermoresponsive heteroarm star-shaped polymers with methacrylate with OEG chains as the hydrophilic arm and PMMA as the hydrophobic arm, using Ru catalyst.
In this study, we first designed the thermoresponsive star-shaped polymer with heteroarm structure based on the methacrylates using living radical polymerization with Ru catalyst and the arm-first method (Scheme 1). We selected diethylene glycol methyl ether methacrylate (DEGMA) and triethylene glycol methyl ether methacrylate (TEGMA) as thermoresponsive moieties, and methyl methacrylate (MMA) as a hydrophobic moiety. For comparison of the star-shaped polymers, the thermoresponsive properties of the linear homopolymers, random copolymers, and block copolymers were also evaluated.
![]() | ||
| Scheme 1 Synthetic route of thermoresponsive heteroarm star polymer via Ru-catalyzed living radical polymerization using the arm-first method. | ||
916
000 g mol−1) in dimethyl formamide (DMF) containing 10 mL LiBr. LCST was measured using the JASCO V-550 ETC-505S and JSSCO V-550 ETC-505T system. The samples for LCST measurement were prepared at 2 mg mL−1 concentration and the transmittance was measured using 500 nm light with a change in temperature rate of 1 °C min−1. Surface contact angles were measured using a goniometer (DM-501Hi, Kyowa Interface Science Co., Ltd, Japan).
:
ethyl acetate, 6
:
4, Rf = 0.4). As a result, the target product was obtained. Yield: 43.4 g (72.5%). 1H NMR (400 MHz, CDCl3, δ): 6.02 (s, 1H), 5.56 (s, 1H), 4.29 (t, J = 4.9 Hz, 2H), 3.74 (t, J = 4.9 Hz, 2H), 3.66 (m, 6H), 3.54 (m, 2H), 3.37 (s, 3H), 1.94 (s, 3H).
800, which was in good agreement with the theoretical value expected from the monomer to initiator initial concentration ratio ([DEGMA]0/[ECPA]0) and the monomer conversion. Separately, PDEGMA with Mn of 17
100 and Đ of 2.83 was synthesized by conventional free radical polymerization with AIBN, as a comparison.
| Entry | Polymer type | DEGMA : MMAa (mol) |
M
n b |
Đ | LCSTc, °C |
|---|---|---|---|---|---|
| a Determined by 1H NMR using the signal integrations of ester methylene and ether methylene of DEGMA and ester methyl of MMA. b Determined by SEC using PMMA standard calibration. c Determined by 50% transmittance at 500 nm light of 0.2 wt% polymer solution. d Determined by unit concentration of the initial reaction solution. e Determined by SEC-RALS. f Insoluble in water. | |||||
| 1 | Homo | 100 : 0 |
15 800 |
1.19 | 26 |
| 2 | Block | 83 : 17 |
17 400 |
1.26 | 19 |
| 3 | Statistical | 83 : 17 |
18 500 |
1.26 | 14 |
| 4 | Star | 89 : 11d |
265 000e |
1.50e | NAf |
Star-shaped PDEGMA was synthesized by polymerization of EGDMA, a linking agent with 10 equivalents to the PDEGMA macroinitiator in the presence of Ru(Ind) complex catalyst and n-Bu3N additive. The star-shaped polymer synthesis was carried out in toluene at 80 °C. After 188 hours of reaction, 82% of the macroinitiator was converted to star-shaped polymers. The star-shaped PDEGMA was purified by precipitation with toluene/hexane to remove the unreacted arm polymers. The obtained star-shaped PDEGMA had Mn of 55
500 by SEC and Mn of 265
000 by SEC-RALS (right angle light scattering), whereby the significant difference in Mn supports the star-shaped polymer formation. Since EGDMA incorporated in the star-shaped PDEGMA is hydrophobic and about 10 mol% of EGDMA to PDEGMA is incorporated, the effect of the hydrophobic EGDMA units on the thermoresponsivity cannot be ignored. Therefore, in addition to PDEGMA, block and statistical copolymers with MMA, corresponding to the structure of the linking moiety cut in half, were synthesized as well. The polymerizations were controlled and resulted in PDEGMA-b-PMMA, with a DEGMA
:
MMA unit ratio of 83
:
17, Mn of 17
400, Đ of 1.26, and P(DEGMA-stat-MMA), with a DEGMA
:
MMA unit ratio of 83
:
17, Mn of 18
500, Đ of 1.26.
For evaluation of the thermoresponsivity of the series of PDEGMA polymers, the LCST was evaluated by transmittance of 500 nm light using 2 mg mL−1 aqueous solution. In this study the LCST is defined as the point at which the transmittance is 50%. Linear PDEGMA, obtained by both living radical and conventional free radical polymerization, dissolved homogeneously at low temperatures, and the transmittance decreased rapidly at 26 °C as the temperature increased. The obtained LCSTs were consistent with the reported values and did not depend on the molecular weight dispersion. As expected, the LCSTs of the P(DEGMA-co-MMA) decreased with incorporation of hydrophobic MMA, and the LCSTs of PDEGMA-b-PMMA and P(DEGMA-stat-MMA) were 19 °C and 14 °C, respectively. This may be because the hydrophobic MMA units of the block copolymers aggregate in aqueous solution; but PDEGMA can still form micelles and elongate, whereas the aggregation of MMA units in statistical copolymers makes it difficult for the PDEGMA chains to hydrate and elongate. In contrast to linear PDEGMA and copolymers with MMA, star-shaped PDEGMA hardly dissolved in water even at low temperatures. Since the content of the hydrophobic units was close to that of the block and statistical copolymers, this difference could be due to a molecular weight effect or a topological effect. Some examples of a decrease in LCST with increasing number of branches in star-shaped polymers compared to linear polymers have been reported previously.24,25
000–25
000 and a narrow polydistribution with Đ < 1.2 (Table 2). The synthesis of star-shaped PTEGMA using the obtained PTEGMA as a macroinitiator also proceeded successfully. After removal of unreacted PTEGMA, star-shaped PTEGMA with Mn of ∼210
000 and with a Đ of 1.31 was obtained by SEC-RALS measurements.
| Entry | Polymer type | TEGMA : MMAa (mol) |
M
n b |
Đ | LCSTc, °C |
|---|---|---|---|---|---|
| a Determined by 1H NMR using the signal integrations of ester methylene and ether methylene of TEGMA and ester methyl of MMA. b Determined by SEC using PMMA standard calibration. c Determined by 50% transmittance at 500 nm light of 0.2 wt% polymer solution. d Determined by unit concentration of the initial reaction solution. e Determined by SEC-RALS. | |||||
| 1 | Homo | 100 : 0 |
22 400 |
1.12 | 52 |
| 2 | Block | 81 : 19 |
24 300 |
1.17 | 46 |
| 3 | Statistical | 83 : 17 |
24 100 |
1.17 | 43 |
| 4 | Star | 90 : 10d |
207 000e |
1.31e | 43 |
The LCSTs of the series of obtained PTEGMA and copolymers were measured. The LCST of the linear PTEGMA was 52 °C, consistent with literature values (Table 2). Block and statistical copolymers containing approximately 20% MMA units had almost the same molecular weight and molecular weight dispersion, but their LCSTs were different and lower than those of the homopolymers, at 46 °C and 43 °C, respectively. This was the same trend as for the LCST measurements of PDEGMA. On the other hand, star-shaped PTEGMA could be dissolved in water and LCST measurements were possible, with a value of 43 °C, which is close to the value for the statistical copolymer. These results indicate that the order of LCST for methacrylate polymers with short ethylene glycol side chains and copolymers with MMA tends to be homopolymer > block copolymer > statistical copolymer ≥ star-shaped polymer.
000–23
000 and Đ of about 1.2 were obtained by systematically changing the initial DEGMA/TEGMA ratio (Table 3). The DEGMA/TEGMA ratio in the obtained copolymers was also close to the initial ratio.
| Entry | DEGMA : TEGMAa (mol%) |
DEGMA : TEGMAb (wt%) |
M
n c |
Đ | LCSTd, °C |
|---|---|---|---|---|---|
| a Determined by 1H NMR using the signal integrations of ester methylene, ether methylene and ether methyl of DEGMA and TEGMA. b Calculated from the results of DEGMA and TEGMA molar composition considering their molecular weight. c Determined by SEC using PMMA standard calibration. d Determined by 50% transmittance at 500 nm light of 0.2 wt% polymer solution. | |||||
| 1 | 100 : 0 |
100 : 0 |
15 700 |
1.19 | 26 |
| 2 | 85 : 15 |
82 : 18 |
14 300 |
1.25 | 32 |
| 3 | 83 : 17 |
80 : 20 |
15 700 |
1.16 | 35 |
| 4 | 73 : 27 |
68 : 32 |
13 600 |
1.15 | 37 |
| 5 | 47 : 53 |
42 : 48 |
14 000 |
1.22 | 41 |
| 6 | 0 : 100 |
0 : 100 |
22 400 |
1.12 | 52 |
The LCSTs were evaluated for the series of P(DEGMA-stat-TEGMA) obtained. As expected, LCST increased with increasing TEGMA content from 26 °C for PDEGMA homopolymer, to 52 °C for PTEGMA homopolymer. In particular, in the range of 15–27% molar content of TEGMA, the LCST could be controlled at 32–37 °C, a value that is near the physiological temperature. The relationship between molar and weight content of TEGMA in P(DEGMA-stat-TEGMA) and LCST is shown in Fig. 1. This relationship is roughly linear, but in regions of low TEGMA content the LCST was slightly higher than predicted by the linear relationship, and the nature of TEGMA tended to be strongly expressed. In addition, when comparing molar content and weight content, weight content tended to be closer to the linear relationship. This result is slightly different from that reported by Yamamoto et al.,15 where a linear relationship between molar content and LCST was observed, but may be due to differences in the molecular weight of the polymer measured and the LCST measured concentration.
![]() | ||
| Fig. 1 Dependence of LCST on TEGMA content for P(DEGMA-stat-TEGMA). Circle: molar content; triangle: weight content. | ||
:
TEGMA = 83
:
17 composition, and hydrophobic PMMA as arm polymers was synthesized. The LCST of this P(DEGMA-stat-TEGMA) is 35 °C, which is near to the physiological temperature. The arm polymer of PMMA was synthesized by living radical polymerization using ethyl 2-bromo isobutyrate as initiator with Ru complexes to obtain a living polymer with Mn of 8200 and Đ of 1.25. The heteroarm star-shaped polymer was synthesized by Ru-catalyzed polymerization of EGDMA from a mixed macroinitiator of P(DEGMA-stat-TEGMA) (Mn of 15
700, Đ of 1.16) and PMMA, in a ratio of P(DEGMA-stat-TEGMA)
:
PMMA = 75
:
25. The ratio of hydrophilic to hydrophobic chains was determined with reference to our previous study of PHEMA/PMMA heteroarm star-shaped polymers.45 In the SEC curve of the reaction solution at 185 hours after the start of the reaction, a new peak appeared on the higher molecular weight side than the macroinitiator, confirming the formation of star-shaped polymers (Fig. 2A). The conversion to star-shaped polymer was roughly calculated from the peak area and found to be 67%. The star-shaped polymer was precipitated by gradually adding hexane to 10 wt% polymer solution in toluene to remove unreacted branch polymers. The Mn of the resulting star-shaped polymers was 72
000 by SEC and 126
000 by SEC-RALS, suggesting the formation of star-shaped polymers even from the large molecular weight difference based on the difference in exclusion volume. The 1H NMR spectrum of the obtained polymers contained both P(DEGMA-stat-TEGMA) and PMMA components, strongly suggesting the formation of heteroarm star-shaped polymers (Fig. 2B). Calculating the ratio of arm polymers from the composition of DEGMA, TEGMA, and MMA in the star-shaped polymer and the degree of polymerization of each arm polymer gave P(DEGMA-stat-TEGMA)
:
PMMA = 73
:
27, which was consistent with the initial ratio (see ESI†). The average number of arms was estimated to be 8.7 from the molecular weight, indicating that this heteroarm star-shaped polymer has about 6.4 arms of P(DEGMA-stat-TEGMA) and 2.3 arms of PMMA.
The obtained P(DEGMA-stat-TEGMA)/PMMA heteroarm star-shaped polymer was insoluble in water and the LCST could not be measured. Therefore, we spin coated this heteroarm star-shaped polymer onto PET film and attempted to evaluate its thermoresponsivity through surface hydrophilicity using the water contact angle. However, measurement of the water contact angle under ambient atmosphere was difficult because water droplets evaporate relatively quickly at 40 °C, which is expected to be above the LCST for this polymer. In addition, hydrophobic PMMA chains are exposed on the surface in the dry conditions under air, since air is hydrophobic, and rearrangement of the arm polymers is expected upon contact with water—which makes correct evaluation difficult. Therefore, the hydrophilicity was evaluated by the contact angle of the captive bubble in water at different temperatures. The contact angle of the captive bubble on the heteroarm star-shaped polymer-coated surface at 20 °C was stable immediately after bubble attachment and was 131 ± 0.6° at 40 s after bubble attachment (Fig. 3). The contact angle of the captive bubble at 40 °C was also stable and almost independent of time, reaching 126 ± 1.9° after bubble attachment, indicating an increase in hydrophobicity. This confirms that the heteroarm star-shaped polymer coating also shows thermoresponsivity, and that a thermoresponsive functional surface can be created simply by coating. When a thick-coated film of this polymer was made using the drop-cast method, it was transparent at low temperatures of 20 °C and cloudy at high temperatures of >40 °C, and this response was reversible (Fig. S18†). This suggests heteroarm star-shaped polymers as a promising material for creating functional surfaces that are insoluble in water, yet thermoresponsive in water.
Footnote |
| † Electronic supplementary information (ESI) available: Schemes S1–S9 for polymer synthesis, Fig. 1, 3, 4, 6, 8, 10, 12, 14, and 16 for SEC curves and 1H NMR spectra of the obtained polymers, Fig. 2, 5, 7, 9, 11, 13, 15, and 17 for UV diagrams, traced by the transmittance with a 500 nm light beam in LCST measurements, and Fig. 18 for photo images of thermoresponsive behavior of heteroarm star-shaped polymer coating. See DOI: https://doi.org/10.1039/d2py01518h |
| This journal is © The Royal Society of Chemistry 2023 |