Miriam
Abad
ab,
Martina
Nardi
c,
Luis
Oriol
ab,
Milagros
Piñol
*ab and
Eva
Blasco
*de
aInstituto de Nanociencia y Materiales de Aragón (INMA), CSIC-Universidad de Zaragoza, Zaragoza 50009, Spain. E-mail: mpinol@unizar.es
bDepartamento de Química Orgánica, Facultad de Ciencias, Universidad de Zaragoza, Pedro Cerbuna, 12, Zaragoza 50009, Spain
cInstitute of Nanotechnology (INT), Karlsruhe Institute of Technology (KIT), Hermann-von-Helmholtz-Platz 1, Eggenstein-Leopoldshafen 76344, Germany
dOrganic Chemistry Institute, University of Heidelberg, In Neuenheimer Feld 270, 69120, Germany. E-mail: eva.blasco@oci.uni-heidelberg.de
eInstitute for Molecular Systems Engineering and Advanced Materials, University of Heidelberg, In Neuenheimer Feld 225, 69120, Germany
First published on 22nd November 2022
Self-assemblies containing the nucleobase analogue 2,6-diacylaminopyridine (DAP) have been successfully prepared for the first time by aqueous seeded RAFT polymerization in high concentrations. For this purpose, a diblock copolymer containing poly(ethylene glycol) (PEG) and DAP polymethacrylate blocks was used as a macro-chain-transfer agent (PEG124-b-PDAP9-CTA) for the polymerization of 2-hydroxypropyl methacrylate (HPMA) in water. From the systematic variation of the degree of polymerization and solid concentration, a phase diagram has been generated that correlates both variables with the morphologies of this new system. Self-assemblies have been characterized by TEM and DLS, observing morphologies from low to high order (from spherical micelles to worms and to vesicles). Self-assembly morphologies are stable for almost a year, except in the case of worms that turn into spherical micelles after a few weeks. In addition, H-bonding supramolecular functionalization of the DAP repeating units during aqueous seeded RAFT polymerization has been examined by functionalization with a cross-linker with four thymine groups. Finally, the loading and the subsequent release of Nile Red have been proven in both supramolecular cross-linked and non-cross-linked self-assemblies.
Among the controlled radical polymerizations suitable for PISA, reversible addition–fragmentation chain-transfer (RAFT) polymerization has been the most widely exploited thanks to metal-free conditions, its high tolerance to functional groups and the possibility to obtain well-defined architectures with predetermined molar masses, low dispersities and end-group fidelity.9,11 Commonly, a macro-chain-transfer agent (macro-CTA) is employed for the PISA polymerization to grow a BC that self-assembles in situ. Depending on the solubility of both the macro-CTA and the monomer, emulsion RAFT polymerization,12 dispersion RAFT polymerization13–18 or seeded RAFT polymerization19 is possible. The latter and more recent one uses an amphiphilic BC macro-CTA that self-assembles in the polymerization medium acting as a seed or nanoreactor for a third block chain extension. Depending on the solubility of the monomer employed, and the resultant polymeric chain, seeded RAFT polymerization can be categorized into different types.19–22
Even though PISA self-assemblies are usually stable in the polymerization medium, the conditions of the environment in which they perform their function (i.e. the presence of non-selective solvents, proteins, surfactants or very dilute media) can compromise their stability. Therefore, covalent cross-linking18 either during polymerization, employing divinyl monomers,23–28 or by either chemically29–32 or photochemically33,34 activated post-polymerization processes has been reported to enhance the nanoparticle stability. However, supramolecular or non-covalent cross-linking has been a less explored alternative despite being an easy and more versatile approach. In addition, its dynamic nature can be advantageous for certain applications like drug delivery. Examples of PISA incorporating non-covalent interactions have been described with either electrostatic,35 host–guest36,37 or hydrogen bonding interactions. In particular, hydrogen bonding interactions have been studied not only as cross-linking interactions38,39 but also as a driver for template interactions,14,16,40,41 and even responsible for upper critical solution temperature (UCST) behavior.42
Among suitable monomers for aqueous dispersion RAFT polymerization, 2-hydroxypropyl methacrylate (HPMA) has been widely studied since it is a water-miscible monomer (up to 13 w/v % at room temperature) that forms a water-insoluble polymer.15 PISA polymerization of HMPA has been approached using several macro-CTAs or hydrophilic stabilizer blocks such as poly(glycerol methacrylate),15,23,27–29,43,44 poly(2-(methacryloyloxy)ethyl phosphorylcholine)26 or poly(ethylene glycol) (PEG)13,17,30,33,43,45–48 or even statistical copolymers like poly(glycerol methacrylate-st-glycidyl methacrylate).31,36
For some time now, our group has worked on the synthesis and self-assembly of linear-linear7,49,50 and linear-dendritic51 amphiphilic BCs containing a PEG hydrophilic block and a hydrophobic one bearing the 2,6-diacylaminopyridine (DAP) unit, which is a nucleobase analogue able to form multiple hydrogen bonds, for different purposes. Furthermore, PEG has been recurrently employed in biomedical applications given that it is non-toxic and able to reduce immunogenicity, which enables the extension of in vivo circulation lifetimes of any encapsulated molecules.52 These DAP-containing amphiphilic BCs exhibited excellent self-assembly behavior forming homogeneous dispersions of micelles or vesicles either by solvent-switching or microfluidics, and their potential as nanocarriers has been evaluated using fluorescent probes,7,49–51 or camptothecin49 and naproxen7 as drug models. The cell viability of these systems was confirmed on several cell lines as well as the pH49 and light-stimulated50 release of the cargoes, in the last case using thymine-containing azocompounds as photoresponsive moieties supramolecularly linked to DAP units. Recently, this outstanding self-assembly behavior has been exploited to process hybrid systems consisting of plasmonic Pd(0) nanosheets, grown inside of polymeric micelles, for photothermal therapy under NIR stimulation.7
In order to further exploit the potential of incorporating nucleobase analogues such as DAP units into amphiphilic BCs, this work explores the preparation of highly concentrated aqueous self-assembly dispersions using the PISA methodology and the supramolecular H-bonding functionalization of the formed self-assemblies. Although there are some examples on the dispersion RAFT polymerization of nucleobases, such as the polymerization of adenine- and thymine-containing monomers in chloroform or dioxane by Kang et al.,14,16 to the best of our knowledge neither nucleobase nor nucleobase analogues have been employed in RAFT-PISA in water. One of the reasons is the often poor water solubility of the nucleobase-containing monomers. Thus, a new strategy has been designed herein to integrate DAP units into a BC which is then employed as a macro-CTA for the aqueous seeded RAFT polymerization of HPMA. Moreover, the feasibility of supramolecular functionalization has been demonstrated using a cross-linker with thymine terminal moieties to induce self-assembly and supramolecular cross-linking in one-pot.
Scheme 1 Synthesis of the PEG124-b-PDAP9-CTA macro-CTA by RAFT polymerization, and PEG124-b-PDAP9-b-PHPMAn by aqueous seeded RAFT polymerization. |
In this way, a diblock copolymer macro-CTA with a PEG and a PDAP blocks was first synthesized in two steps (Scheme 1) by RAFT polymerization. Commercial PEG monomethyl ether (PEG124-OH, 5450 g mol−1) was first conjugated with 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoic acid by a Steglich esterification reaction to obtain the corresponding PEG124-CTA. This chain-transfer agent was chosen since it is suitable for (meth)acrylate polymerization.53,54PEG124-CTA was characterized by GPC (Fig. S1†) and the successful incorporation of the CTA was verified by 1H NMR spectroscopy (Fig. S2†). In a second step, the BC PEG124-b-PDAP9-CTA was prepared by RAFT polymerization (Scheme 1) of the methacrylic monomer mDAP from PEG124-CTA.55 Based on our experience, the target degree of polymerization of the PDAP block was limited to 10 to ensure an adequate water compatibility of the resulting BC macro-CTA. The experimental degree of polymerization and average molar mass (Mn) of the resulting diblock copolymer were determined by 1H NMR spectroscopy (Fig. S3†) as 9 and 9440 g mol−1, respectively. The polymer was also characterized by GPC and a low polydispersity was found (Đ = 1.18) (Fig. S1†).
The resulting BC, PEG124-b-PDAP9-CTA, was directly dispersed in water forming transparent solutions up to 10 g of polymer per 100 mL of water. Due to its amphiphilic character, the possible self-assembly in water was evaluated by transmission electron microscopy (TEM) (Fig. 1) and dynamic light scattering (DLS) (Fig. S4†). Short worms coexisting with a small population of spherical micelles of 15 ± 4 nm diameter were observed by TEM at 0.1 g per 100 mL polymer concentration (Fig. 1a). The self-assembly behavior of PEG124-b-PDAP9-CTA in mixtures of water and HPMA was also studied simulating the aqueous RAFT polymerization conditions (T = 50 °C). Two mixtures containing [HPMA]/[PEG124-b-PDAP9-CTA] = 100 and 300 molar ratios at a solid content of 10 g in 100 mL of water were evaluated and the values corresponded to the molar ratios and concentration feed in the aqueous RAFT polymerization (see below). The TEM images indicated that worms were shortened, and spherical micelles of 15 ± 4 nm diameters were predominant in the first mixture (Fig. 1b). However, by increasing the concentration of HPMA, it was found that the worms disappeared and spherical micelles were larger in size (27 ± 10 nm) and dispersity (Fig. 1c). DLS measurements of the self-assemblies were also performed at the polymerization temperature (50 °C) and it was observed that the presence of HPMA decreased the apparent Dh (Fig. S4†). Therefore, when the macro-CTA and HPMA were dispersed together in water, the initial PEG124-b-PDAP9-CTA preferentially formed spherical micelles.
The aqueous seeded RAFT polymerization of HMPA using PEG124-b-PDAP9-CTA (Scheme 1) was initiated by 2,2′-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (VA-044) at 50 °C. A 0.3 molar ratio between the initiator and macro-CTA ([VA-044]/[PEG124-b-PDAP9-CTA]) was employed. This ratio was previously reported as optimum for aqueous RAFT-PISA of HMPA using PEG124-CTA to obtain well defined copolymers with relatively low dispersity and minimal homopolymer contamination.13 Polymerization was maintained for 5 h.
The influence of the polymer concentration and the length of the hydrophobic segments on the self-assembling properties was investigated by performing three series of experiments, x = 1, 2 and 3, where the target degree of polymerization given by the [HPMA]/[PEG124-b-PDAP9-CTA] ratio was approx. n = 100, 200 and 300, respectively. For each series, polymerization was performed at different solid concentrations (c = 10, 15, 20 and 25 expressed as grams of solids per 100 mL of water). 25 g per 100 mL was determined to be the maximum concentration at which PEG124-b-PDAP9-CTA was well dispersed in water before precipitation. The experiments were coded as c − x, where c refers to the solid concentration and x refers to the series of polymers. In all cases very high HPMA conversion values (≥98%) were obtained (Table S1†), as calculated by 1H NMR (Fig. S6†), using DMF as an internal standard.17
Polymers were analyzed by GPC (Fig. 2, S7 and Table S1†). GPC traces of the prepared polymers showed similar average molar masses for BCs with PHPMA of comparable length prepared at different polymer concentrations (Fig. 2). The dispersity values were in all cases between 1.31 and 1.45, higher than that of PEG124-b-PDAP9-CTA (Đ = 1.18). Nonetheless, it was observed that combining high target PHPMA degrees of polymerization and low solid concentrations favored the appearance of a small shoulder at higher elution times. GPC measurements were carried out at different polymer concentrations to dismiss the presence of self-assemblies in the eluent. Thus, shoulders should be most likely attributed to the presence of residual PEG124-b-PDAP9-CTA44,46 due to a relative low degree of uncontrolled polymerization at higher PHPMA degrees of polymerization and lower solid concentration.
Fig. 2 GPC chromatograms of series x = 1–3, polymerized at c = 10, 15, 20 and 25 solid concentrations. Eluent: DMF (LiBr 50 mM). Detector: UV (290 nm). |
The morphology of the self-assemblies prepared by aqueous seeded RAFT polymerization was identified by TEM and cryo-TEM while the average hydrodynamic diameters (Dh) and polydispersity indexes (PDI) were determined by DLS (Table 1). The resulting phase diagram is shown in Fig. 3.
Sample | M n (kDa) | Hydrophilic/hydrophobic ratiob | D h (PDI)c (nm) | TEM sized (nm) | Morphology |
---|---|---|---|---|---|
a Average number molar mass (Mn) calculated considering for PEG124-b-PDAP9-CTAMn = 9440 g mol−1 (estimated by 1H NMR) and the PHPMA degree of polymerization. b Hydrophobic/hydrophilic weight percentage ratio estimated considering the PEG block as the hydrophilic part and the PDAP9-b-PHPMAn segment as the hydrophobic part. c Average Dh values and PDI provided by Zetasizer software, from the intensity particle size distribution recorded by DLS. d TEM size data were reported as the mean ± SD (standard deviation) of a 150 measurements histogram. e Mean size and SD could not be reported since the histogram obtained did not fit to a Gaussian curve. | |||||
10-1 | 26.0 | 21/79 | 39 ± 9 (0.02) | 25 ± 6 | Spherical micelles |
10-2 | 40.3 | 13/87 | 70 ± 20 (0.07) | 44 ± 9 | Spherical micelles |
10-3 | 58.2 | 9/91 | 164 ± 57 (0.10) | 55–350e | Unilamellar vesicles |
15-1 | 24.6 | 22/78 | 40 ± 11 (0.06) | 29 ± 7 | Spherical micelles |
15-2 | 41.0 | 13/87 | 326 ± 178 (0.29) | 33 ± 6 | Worms (+spheres) |
15-3 | 57.9 | 9/91 | 883 ± 422 (0.19) | 220–1750e | Oligolamellar vesicles |
20-1 | 25.5 | 21/79 | 38 ± 12 (0.10) | 21 ± 6 | Spherical micelles |
20-2 | 40.7 | 13/87 | 436 ± 169 (0.37) | 32 ± 9 | Worms (+spheres) |
20-3 | 56.5 | 10/90 | 949 ± 489 (0.24) | 100–1500e | Oligolamellar vesicles |
25-1 | 24.5 | 22/78 | 41 ± 11 (0.05) | 25 ± 6 | Spherical micelles |
25-2 | 40.2 | 14/86 | 883 ± 551 (0.47) | 37 ± 8 | Worms (+spheres) |
25-3 | 54.7 | 10/90 | 906 ± 540 (0.34) | 95–1500e | Oligolamellar vesicles |
For series x = 1, having an approx. target polymerization degree of n = 100, turbid but fluid homogeneous dispersions of micelles were obtained for all tested polymerization concentrations (i.e. from c = 10 to 25 g solids per 100 mL of water) with average Dh values around 40 nm which were larger than those of PEG124-b-PDAP9-CTA, and low PDI (<0.1). Taking these observations as a starting point, transitions to more ordered morphologies from spherical micelles-to-worms-to-vesicles were detected on increasing both the length of the PHPMA block, i.e., the hydrophobic content of the final BCs, and the total solid concentration.
For instance, when fixing the solid concentration at c = 10 g per 100 mL but increasing the target degree of polymerization, an increase of the turbidity of the collected dispersions was observed with the naked eye. Accordingly, for 10-2 spherical homogeneous micelles of a larger size were self-assembled, with the average Dh increasing from 39 ± 9 nm for 10-1 to 70 ± 20 nm for 10-2 (Fig. S8†). Then, unilamellar vesicles were identified by cryo-TEM for 10-3 (Fig. 4) with sizes ranging from 55 to 350 nm (average Dh = 164 ± 57 nm) and a membrane thickness of 21 ± 2 nm. For 10-3, the remaining spherical micelles were also observed by TEM.
Fig. 4 Cryo-TEM images from PEG124-b-PDAP9-b-PHPMAn dispersions of series x = 3, obtained at different solid concentrations (c = 10, 15, 20 and 25). |
Considering higher solid concentrations (c = 15, 20 and 25 g per 100 mL) and high target degree of polymerization (series x = 2 and 3), opaque white viscous dispersions with intermediate or even more complex and mixed self-assembly morphologies were produced. For 15-2, 20-2 and 25-2, worms of approx. 35 nm cross section were predominantly detected in TEM images with some residual spherical micelles. The high viscosity of dispersions with a soft gel like appearance can probably be associated with a network formation due to entanglements of the worms.57 By DLS (Fig. S8†), broad size distributions with large PDI values were registered. Nonetheless, DLS data should be handled with caution for worm-like particles since Dh values are estimated under the assumption that the particles exist in solution as compact spheres.
For samples of series x = 3, more complex morphologies were observed by TEM (Fig. 3) and cryo-TEM (Fig. 4) above a concentration of 10 g per 100 mL, consisting of a mixture of unilamellar and oligolamellar vesicles, or vesicles within vesicles, with sizes ranging from a few hundred nm to a few μm and 25–30 nm membrane thickness. Vesicles with sizes above 1 μm appeared as broken or folded even in cryo-TEM. The folding of such large vesicles in cryo-TEM is not unusual since the vitrified ice layer should only be around a few hundred nm. In addition, some worms and intermediate morphologies of worm-to-vesicle transitions such as wormballs and jellyfish-like geometries were observed (Fig. S9†).15
Despite the presence of PDAP blocks, the results obtained from the morphological characterization of PEG124-b-PDAP9-b-PHPMAn self-assembly dispersions prepared by aqueous seeded RAFT polymerization were in accordance with the ones from BCs prepared by aqueous dispersion RAFT polymerization, using PEG as the macro-CTA and HPMA as the monomer.13,17
The stability of the dispersions upon storage was evaluated by DLS up to 11 months (Fig. S10†). Those dispersions with self-assembled spherical micelles (10-1, 15-1, 20-1, 25-1 and 10-2) and unilamellar vesicles (10-3) were stable as concluded from the registered DLS curves, with only a slightly increase in average Dh and PDI for samples 10-1 and 15-1 due to some aggregation of the micelles as observed by TEM (Fig. S11†) after 11 months. For those samples containing oligolamellar vesicles or vesicles within vesicles (15-3, 20-3 and 25-3) only slight variations were observed along the time. However, a clear evolution was observed after 6 weeks for dispersions containing worms (15-2, 20-2 and 25-2) with a remarkable decrease of the apparent Dh. However, DLS measurements taken at the 12th week were similar to those of the 6th week (Fig. S12a†). After 12 weeks, TEM images showed a large population of spherical micelles coexisting with short worms (Fig. S12b†). This suggests the worm dissociation into cylindrical and spherical micelles, which might be more thermodynamically stable morphologies.13,43 No significant further evolution of the samples was observed after 11 months.
In order to incorporate the thymine derivative T4 into the system, one-pot seeded polymerization and supramolecular cross-linking were carried out. In particular, we performed an analogous experiment on a 10-1 sample targeting a degree of polymerization of approx. 100 (series x = 1) and a final polymer concentration c = 10 (resulting material coded 10-1·T4) using a T4:PEG124-b-PDAP9-CTA molar ratio of 2.2:1 (i.e. a 1:1 thymine:DAP ratio). Because T4 is not soluble in water, it was incorporated into a small amount of DMF employed as an internal standard in the polymerization process (see details in the Experimental section). Prior to seeded aqueous polymerization, the influence of T4 on the initial self-assemblies of PEG124-b-PDAP9-CTA and PEG124-b-PDAP9-CTA and HPMA mixture was tested by TEM (Fig. S13†) observing that T4 induced the transformation to shorter worms and more spherical micelles in the first case while only spherical micelles were observed if HPMA was present. Polymerization was conducted to a high conversion (98%; Table S1†) similar to the 10-1 sample.
This time the envisaged self-assembly and supramolecular cross-linking resulted in a milky appearance dispersion for 10-1·T4 in contrast to the translucent dispersion collected for 10-1. GPC analysis (Fig. S14†) gave a low dispersity value, Đ = 1.31, in analogy to 10-1. Notwithstanding, GPC curves show two polymer distributions, one of them at the same elution time as the corresponding non-cross-linked sample, and another at higher elution time. This suggests that the HPMA polymerization is hindered to some extent by the presence of T4. By TEM (Fig. 5c), spherical micelles with a diameter of 21 ± 3 nm, smaller in size than the corresponding non-cross-linked ones, were observed, and they tend to aggregate. These micelles coexist with big spheres having sizes between 125 and 200 nm which seemed to have a compact and solid core as was suggested by cryo-TEM (Fig. 5d). These big spheres’ contribution in DLS shifted the mean size distribution to a higher Dh value (Dh = 137 ± 55 nm) (Fig. 5e). Therefore, the presence of T4 during the polymerization seemed to affect the polymerization and consequently the morphology of the self-assemblies formed.
Having established the conditions for the preparation of supramolecular cross-linked self-assemblies in water, the influence of cross-linking on the encapsulation and release of small molecular cargoes was investigated. Nile Red (NR) was selected as a hydrophobic molecular fluorescent probe. First, NR was encapsulated by diffusion in 10-1 and 10-1·T4 samples. NR loaded dispersions were characterized by DLS and TEM (Fig. S15†). By DLS only one size distribution was observed in both cases, very similar to the corresponding plain samples. Also by TEM, similar morphologies were observed with only a slight increase in the average size for 10-1 + NR, from 25 to 29 nm when compared to 10-1. As was seen by fluorescence spectroscopy (Fig. 5g and h), a higher amount of NR was encapsulated into 10-1·T4 than into 10-1, around 1.4 times more. To evaluate the NR release, both dispersions were dialyzed against a large water volume following NR fluorescence evolution as it is related to the NR still encapsulated. As can be seen in Fig. 5f, NR release was slower for 10-1·T4 than for 10-1, which evidences the higher stability of supramolecular cross-linked self-assemblies compared to non-cross-linked ones.
Dynamic Light Scattering (DLS) measurements were carried out in a Malvern Instrument Nano Zs (Malvern, Worcestershire, UK) using a He–Ne laser with a 633 nm wavelength and a detector angle of 173° at 25 °C. The aqueous self-assembly dispersions were measured at an approximately 1.0 mg mL−1 concentration, and hydrodynamic diameters (Dh) were given as an average of three measurements on each sample to ensure reproducibility. Transmission Electron Microscopy (TEM) analysis was performed using a FEI Tecnai T20 microscope (FEI Company, Waltham, MA, USA) operating at 200 kV. TEM samples were prepared adding 10 μL of each self-assembly dispersion at an approximately 1.0 mg mL−1 concentration on a continuous carbon film-copper grid, and the excess was removed by capillarity using filter paper. Then, the grids were stained with uranyl acetate (1% aqueous solution), removing the excess again by capillarity using filter paper. The grids were dried overnight under vacuum. Cryogenic Transmission Electron Microscopy (Cryo-TEM) analysis was performed in a JEM-2011 microscope (Jeol Europe SAS, Croissy-sur-Seine, France) operating at 80 kV. For cryo-TEM, holey carbon film-copper grids previously ionized using a plasma cleaner were employed. A droplet was placed onto the grid, and sample vitrification was automatically performed using FEI Vitrobot and liquid ethane. Samples were kept under liquid nitrogen with a Gatan TEM cryo-holder (FEI Company). Fluorescence emission spectra were obtained using a Fluorolog FL3-11 spectrometer (HORIBA ABX SAS, Madrid, Spain), with a Front Face accessory.
PEG124-CTA (0.52 g, 0.10 mmol), monomer mDAP (0.36 g, 0.95 mmol), and AIBN (2.35 mg, 0.014 mmol) were added to a crimp vial and dissolved in dioxane (2.2 mL). The resulting solution was purged for 20 min with Ar and then placed into a preheated oil bath at 75 °C. After 6 h, the reaction mixture was cooled down with an ice bath and exposed to air. The crude product was precipitated twice in cold diethyl ether. The solid was centrifuged and dried under vacuum overnight. PEG124-b-PDAP9-CTA was obtained as a slight yellow powder. Yield: 83%. Conversion: 93%. FT-IR (KBr disk, cm−1): 3318, 2885, 1965, 1734, 1695, 1585, 1517, 1448, 1359, 1343, 1282, 1243, 1150, 1114, 1061, 964, 947, 842, 803. 1H NMR (400 MHz, CDCl3) δ (ppm): 8.97–8.23 (19H), 7.96–7.50 (29H), 4.42–4.05 (37H), 3.83–3.43 (528H), 3.37 (3H), 2.89–2.59 (37H), 2.44–2.27 (19H), 1.34–0.78 (65H). GPC (DMF): Mn = 32910 g mol−1; Đ = 1.18.
By changing the length of the PHPMA block (series x = 1, 2 and 3) and the solid concentration (from 10 to 25 g per 100 mL), a phase diagram of these new PEG124-b-PDAP9-b-PHPMAn formulations has been constructed. TEM and DLS studies indicated that the aqueous seeded RAFT polymerization of HPMA led to aqueous self-assembly dispersions with diverse morphologies (spherical micelles, worms and vesicles), which depended on the length of the PHPMA block and solid concentration. The resulting self-assembly dispersions remain almost stable at least for 11 months, except in the case of worms’ morphology, in which a transition to spherical micelles was progressively observed.
Incorporation of nucleobase analogue DAP units allows the supramolecular functionalization with thymine complementary derivatives by triple H-bonding. This possibility has been initially evaluated by incorporating a cross-linking agent with four terminal thymine groups (T4) during aqueous seeded RAFT polymerization of HPMA. It was found that T4 influenced the polymerization and the self-assembly morphologies. In addition, NR was successfully encapsulated as a hydrophobic molecular fluorescent probe by diffusion in both non-cross-linked and supramolecular cross-linked self-assemblies. For the latter, a larger amount of NR could be encapsulated as well as a slower release was also observed. These preliminary results suggest a higher stability of the supramolecular cross-linked self-assemblies, evidencing the potential use of the system as nanocarriers.
Footnote |
† Electronic supplementary information (ESI) available: mDAP solubility tests; Fig. S1–S16 and Table S1. See DOI: https://doi.org/10.1039/d2py01250b |
This journal is © The Royal Society of Chemistry 2023 |