Open Access Article
Melik Oksuz and
H. Yildirim Erbil
*
Department of Chemical Engineering, Gebze Technical University, Gebze 41400, Kocaeli, Turkey. E-mail: yerbil@gtu.edu.tr
First published on 14th May 2018
Although many factors are considered to improve the properties of graphene filaments, there is no report in the existing literature on the effect of the temperature of the coagulation bath to the mechanical properties of graphene oxide filaments obtained in the wet-spinning process and also to the mechanical and electrical properties of the resulting graphene filaments after reduction. In this study, the effect of the temperature of the isopropanol coagulation bath during wet-spinning of graphene filaments on their final properties after formation was investigated and it was found that the decrease of the coagulation bath temperature resulted in more compact filaments having better mechanical properties for both graphene oxide and corresponding reduced graphene filaments. The best tensile strength and Young's modulus values were obtained in isopropanol coagulation bath which was kept at 15 °C. On the other hand, the types of the chemical reduction agents which can provide better electrical conductivity to graphene filaments after reduction were also investigated and it was determined that the use of hydriodic acid/acetic acid mixture resulted in graphene filaments having the best electrical conductivity (1.28 × 104 S m−1) and also tensile strength (234 ± 26 MPa) values. The addition of acetic acid into hydriodic acid increased the tensile strength 26% when compared with the plain HI treatment. Both electrical conductivity and tensile strength results were higher than most of the previously reported values of the wet-spun neat graphene filaments in the literature.
Two methods are generally used to obtain GFs: (i) wet-spinning of an aqueous graphene oxide (GO) dispersion into a coagulation bath to obtain GO filaments which are then reduced to GFs by several methods; (ii) application of a hydrothermal reaction where an aqueous GO dispersion is injected into a glass tube and then subjected to thermal annealing (∼230 °C) to obtain the GF directly.23 This method can be also performed at low temperature (∼80 °C) in a plastic tube where a chemical reduction agent is added into GO dispersion before injection.24 It was reported that GFs obtained by the hydrothermal method had poor mechanical properties and lower electrical conductivity than that of the GFs obtained by the wet-spinning method. Hydrothermal method was also found to be less suitable for large scale filament production.11,23,24 Some other methods, such as chemical vapor deposition,25 electrophoretic self-assembly26 have also been reported in the literature to obtain GFs but they were reported to be more expensive when compared with the wet-spinning method.
Some additives were used to improve the properties of the resultant GFs. For example, Xu et al. obtained stretchable conductor GFs by adding silver nanowires to GO dispersion.27 Fang et al. produced hybrid fiber having fire-resistant properties by adding montmorillonite to system.28 Wu et al. introduced hydrophilicity and antifouling property to polymeric membranes by using GO/water as coagulation bath.29
Cao and Xu reported that wet spun GFs production can be made by only using the GO dispersions having the liquid crystal property which can be obtained only at high GO concentrations in water.30 Thus, the increase of GO concentration in water dispersion by centrifuging is a necessary step before the wet-spinning. There are mainly two stages in the wet-spinning process: (i) concentrated GO dispersion is injected into a coagulation bath to form the graphene oxide filaments (GOFs), then these filaments are removed from the bath and dried; (ii) dried GOFs are reduced via thermal annealing or with chemical reduction methods into GFs which are electrically conductive and mechanically strong enough to be used in weaving.
At present, wet-spinning method to obtain GFs is the most popular method as displayed in the increasing number of publications using this process by several groups worldwide. It was determined that the properties of the final GFs are directly affected by the properties of used GOFs.31–34 On the other hand, the type of the coagulation bath which is used in wet-spinning is another important parameter for the GOFs product. Although many different chemicals such as amine solutions,35 sulfuric acid and chitosan solution36 were reported to be used as the coagulation bath during wet-spinning, only three types of coagulation baths were commonly preferred in most of the publications. These are aqueous ionic (Na+, K+, Ca++, Mg++, Cu++) solutions7,33,36 aqueous cationic surfactant (CTAB) solutions8,34 and some organic solvents like ethyl acetate, methyl acetate, isopropanol, ether and acetone.13,27,32,36
When ionic or surfactant containing coagulation baths are used then the obtained GOFs have to be kept in the bath for long durations (∼30 min) to complete the inter-diffusion process of ions and surfactant molecules between the GO layers in the filaments during self-assembly process.33,34,37 The interactions between GO platelets are weak for short filament immersion times and the resultant GOFs have poor mechanical properties. Another problem is the presence of the cationic surfactant molecules in the final GFs, which affects their electrical conductivity adversely. It was reported that the use of organic solvents as coagulation baths resulted in GFs having good mechanical and electrical properties.11,13,32 As a consequence of these experimental findings, only solvent based coagulation baths were used to produce GFs in a pilot plant study.11
Many parameters affecting the mechanical properties of GOFs and GFs were investigated previously in the literature and it was determined that the increase of the GO concentration in the aqueous dispersion resulted in an increase of the mechanical resistance of the obtained GOFs due to better interaction between the GO layers in a confined volume. The use of graphite powders having large particle sizes as the starting raw material for the GO production resulted in mechanically more resistant and electrically conducting GFs when compared with the GFs obtained by using graphite powders having small particle sizes. The presence of large interaction areas between the large GO platelets forms strong filaments.31 On the contrary, some authors suggested that better mechanical properties of GFs could be obtained by mixing both small (30%) and large (70%) GO particles in the doping GO dispersion, since small GO plates would fill the voids between the large ones during the GO filament formation process.34 On the other hand, it was also reported that the mechanical and electrical properties of the filaments could be improved by the application of an optimum tension to GOFs during their production in the coagulation bath.11,32,33
Many factors have been considered to improve the properties of neat GFs when the wet-spinning system was used up to now. However, there was no report in the existing literature on the effect of the temperature of the coagulation bath to the mechanical and electrical properties of GOFs and GFs in the wet-spinning process to the best of our knowledge. It is hypothesized that the effect of temperature during the coagulation step should be an important parameter in the wet-spinning process to affect the mechanical properties of GOFs since it will change the inter-diffusion rate between the water molecules present in the GO dispersion and solvent molecules in the bath and thus will affect the GO platelet self-assembly process. In this work, we investigated the effect of the temperature of an organic solvent (isopropanol) coagulation bath to the mechanical properties of GOFs and, also to the electrical and mechanical properties of GFs obtained after reducing these GOFs chemically. It was determined that the decrease of the coagulation temperature resulted in better mechanical properties for both GOFs and GFs. In addition, we investigated the effect of the types of the chemical reduction agents to improve the electrical properties of GFs and found that the use of hydriodic acid/acetic acid mixture resulted in the GFs having the best electrical and mechanical properties.
:
1 mixture of H2SO4 (200 mL)/H3PO4 (40 mL) and mixed with a magnetic stirrer for 15 min. Then, 25 g KMnO4 was slowly dissolved in the acid-graphite mixture, which were cooled to 10 °C with the aid of a cooling jacket to avoid the explosion risk for 75 min. After the addition of KMnO4, the green mixture was heated up to 40 °C to carry out the oxidation of graphite under stirring in a water bath. After two hours, the mixture turns into a viscous slurry, which was stirred for a further 2.5 hours by using a Teflon rod (in every 7 min). A viscous brown mixture was obtained after 4.5 hours of the oxidation reaction and cooled down to room temperature. Later, a mixture of 600 mL of cold water with 40 mL of 35 wt% H2O2 was slowly added into the viscous mixture and the color of mixture turned from brown to yellow during this stage. The final mixture was left overnight at room temperature and then, GO was separated from the mixture with the aid of a centrifuge at 13
500 rpm. GO cake was washed with 1 L H2SO4 solution (5 wt%) and centrifuged repeatedly after washing with water until the pH value of the supernatant was ∼5. Finally, pure GO cake was dispersed in 2 L of distilled water and aqueous GO dispersion was centrifuged at 3000 rpm for 15 min to separate un-exfoliated graphite oxide and un-oxidized graphite particles. Aqueous GO dispersion (supernatant) was collected in a flask after centrifugation and stored till use for wet-spinning. 1.40 ± 0.05 g of GO per g graphite was obtained with this synthesis procedure.
500 rpm. A wet-spinning system with a rotating bath was used for the production of GO filaments (Fig. 1). GO dope was injected into the coagulation bath at a rate of 0.25 mL min−1 through a motorized nozzle having an inner diameter of 440 μm. Coagulation bath was rotated at a speed of 12 rpm during the GO injection. The nozzle was about 3 cm away from the center of rotating bath. Isopropanol and acetone solvents were used as coagulation baths at room temperature. In further experiments, isopropanol temperature was kept constant at 5, 15, 25 and 35 °C in order to investigate effect of the temperature of the coagulation bath on the mechanical properties of wet-spun GOFs. These experiments were performed in a climatic chamber which can cool down to −30 °C (Memmert CTC 256), to avoid temperature changes (Fig. 1). GO filaments were kept immersed in the coagulation bath for only 2 min, then removed from the bath and placed horizontally on a polypropylene frame where they are adhered with a pressure sensitive tape after slightly straightening and dried at room temperature.
O groups in the ∼1720 cm−1 region, C–O–C groups in the ca. 1370 cm−1 region, C–O groups in the ca. 1050 cm−1 region and C
C groups in the 1620 cm−1 region show the presence of hydroxyl, epoxide, carbonyl and carboxyl groups and also the un-oxidized C
C bonds. The presence or absence of the liquid crystallinity was checked by using a Polarized Optical Microscope (POM) and it was determined that concentrated aqueous GO dope (13 mg mL−1) has liquid crystalline properties. An indicative POM image of the GO dope is shown in Fig. 2d where the orientation of the GO plates and the double diffracted structures are easily seen to demonstrate the presence of liquid crystallinity.
![]() | ||
| Fig. 2 (a) XRD patterns of graphene oxide, inset: XRD pattern of graphite; (b) DSC curve of GO (c) FTIR-ATR spectra of GO; (d) POM images of GO dope. | ||
Acetone is one of the most commonly used solvent to remove water from the GO filament during the production of wet spun GFs at much higher rates compared to other solvents given in the literature.13,18,36 In this study, IPA was used to remove water from the filament with a much lower rate compared to acetone and it was found that GOFs which were obtained in an IPA bath resulted in higher tensile strength and smaller cross-sectional areas (giving more dense filaments) than that of the filaments obtained from the acetone bath as seen in Table 1. It is possible that low tensile strength GOFs were produced when acetone was used as the bath because of the more rapid inter-diffusion rate between water and acetone molecules than that of the inter-diffusion rate between water and isopropanol molecules. The increase in the mass transfer rate resulted in filaments having longer spacing between GO platelets showing poor mechanical properties.32 Indeed, the larger cross-sectional areas of GOFs obtained by the acetone coagulation bath showed a more loose filament structure. Consequently, IPA coagulation baths which gives mechanically stronger GOFs were used for the subsequent bath temperature effect experiments.
| Coagulation bath solvent | Cross section area (μm2) | Tensile strength (MPa) | Elongation at break (%) |
|---|---|---|---|
| Acetone | 2281 ± 91 | 124 ± 13 | 5.0 ± 1.2 |
| Isopropanol | 2194 ± 294 | 156 ± 15 | 5.2 ± 0.6 |
![]() | ||
| Fig. 3 (a) The paper frames used during the tensile tests; (b) SEM image of GOF@25°-IPA sample after the rupture during the tensile test to calculate their cross-section. | ||
Cross-section areas, tensile strengths and elongation at break values of GOFs are given in Table 2. It was determined that better filament tensile strengths and Young's modulus values were obtained when cold isopropanol coagulation baths were used. It is possible that the decrease in the bath temperature resulted in a slower inter-diffusion rate between water and isopropanol molecules and the decrease in the mass transfer rate produces GOFs having less spacing between the graphene oxide platelets in the filament. The contraction in the filament structure resulted in improved mechanical properties. Similar findings were also reported in the published works which were investigating the effect of temperature of coagulation baths on the mechanical properties and morphology of polyacrylonitrile fibers.44,45 As seen in Table 2, the cross-sectional areas deceased with the decrease of the bath temperature indicating the compact structure of GOFs after wet-spinning.
| Sample | Cross section area (μm2) | Tensile strength (MPa) | Elongation at break (%) | Young's modulus (GPa) |
|---|---|---|---|---|
| GOF@5°-IPA | 1962 ± 142 | 161 ± 11 | 5.2 ± 0.5 | 15.4 ± 4.4 |
| GOF@15°-IPA | 2014 ± 176 | 181 ± 23 | 5.3 ± 0.5 | 17.3 ± 5.5 |
| GOF@25°-IPA | 2194 ± 294 | 156 ± 15 | 5.2 ± 0.6 | 14.1 ± 3.7 |
| GOF@35°-IPA | 2315 ± 126 | 147 ± 9 | 5.2 ± 0.4 | 12.0 ± 3.3 |
SEM images of the surfaces of GOFs under different magnifications are given in Fig. 4. The GOFs sample obtained from the coagulation bath having the highest temperature (GOF@35°-IPA) had a very loose filament structure with the widest diameter and largest cross-sectional area, whereas the GOFs sample obtained with the lowest bath temperature (GOF@5°-IPA) had a very contracted filament structure having the smallest cross-sectional area as seen in Fig. 4 and Table 2. It was found that the structural properties of GOFs affected to their tensile strength results. The most compact filament structure resulted in the highest tensile strength and Young's modulus value indicating that the use of coldest IPA coagulation bath should be favored to obtain the best mechanical properties. However, GOF@5°-IPA sample was an exception since its mechanical properties, especially tensile strength (161 ± 11 MPa), was slightly lower than that of the GOF@15°-IPA sample (tensile strength = 181 ± 23 MPa) although the bath temperature was 10° higher. A possible explanation for this point is that the inter-diffusion rate during water-isopropanol exchange was very slow at 5 °C and our constant immersion duration of 2 min in the coagulation bath at this temperature was not enough to finish the GO platelet assembly process in the filament. In order to check the validity of this idea that the constant 2 min period may not be enough for the 5 °C experiments, we extended the immersion time up to 15 min in IPA and obtained GOFs having much better mechanical properties (tensile strength: 189 ± 26 MPa, elongation at break: % 5.1 ± 0.9 and Young's modulus = 18 ± 3 GPa). This result indicates that a duration of two min is not enough for the 5 °C experiments. However, the increase of filament immersion time in the bath is generally a disadvantage for a commercial continuous wet-spinning process. For this reason, we selected GOF@15°-IPA sample, which was kept only for 2 min at 15 °C in the bath to have the optimum mechanical properties and can be used for any scale-up experiments.
![]() | ||
| Fig. 4 SEM images of the surface of GOFs under different magnifications: (a–c) GOF@35°-IPA; (d–f) GOF@25°-IPA; (g–i) GOF@15°-IPA; (j–l) GOF@5°-IPA | ||
| Chemical reduction agent | Reduction temperature (°C) | Cross section area (μm2) | Tensile strength (MPa) | Elongation at break (%) | Young's modulus (GPa) | Electrical conductivity (S m−1) |
|---|---|---|---|---|---|---|
| Hydrazine monohydrate | 90 | 3184 ± 19 | 33 ± 6 | 2.4 ± 1.4 | 4.2 ± 1.5 | 0.09 ± 0.03 × 104 |
| Hydriodic acid | 80 | 1537 ± 143 | 178 ± 34 | 6.3 ± 0.8 | 17.0 ± 4.1 | 0.90 ± 0.05 × 104 |
| Ascorbic acid | 90 | 2279 ± 4 8 | 141 ± 12 | 4.2 ± 2.3 | 20.6 ± 1.5 | 0.24 ± 0.02 × 104 |
| HI/AAc | 40 | 1471 ± 115 | 200 ± 37 | 5.7 ± 0.9 | 21.0 ± 2.7 | 1.20 ± 0.07 × 104 |
It was found that graphene filaments having the best tensile strength and Young's modulus values were obtained from the dried GOF@25°-IPA filaments when HI/AAc mixture was used as the chemical reducing agent. A tensile strength value of 200 ± 37 MPa was found which was higher than most of the previously reported GFs that was reduced by using only chemical agents.7,8,16,24,46 Although a very high tensile strength value of 501 MPa was reported for GFs in the existing literature which was reduced by using only chemical agents,33 this method has some drawbacks since the filament immersion time in the bath (ca. 30 min) is much longer than ours (2 min).
GFs having the most porous filament structure and the worst mechanical properties were obtained when hydrazine monohydrate was used as the reducing agent probably due to the adsorption of gases formed during the reduction reaction.47 On the contrary, the most compressed filament structure, giving the best mechanical properties was obtained when HI/AcA mixture was used as seen in SEM images (Fig. 5a and b). It is interesting that the inclusion of acetic acid into hydriodic acid increased the tensile strength 26% when compared with the plain HI solution. Similarly, Young's modulus values of GFs increased by 24% after HI/AAc reduction as compared with HI. Other reducing agents resulted in more loose filament structures in the following order: HI < AsAc < Hdz. The use of ascorbic acid also resulted in a loose GFs structure. Electrical conductivity results of GFs are given in Table 3. The best result was obtained when HI/AAc mixture was used as the chemical reducing agent for the dried GOF@25°-IPA filament (1.20 × 104 S m−1) which is much higher than most of the electrical conductivity values of (0.03–0.86 × 104 S m−1) of wet-spun neat GFs reported in the literature.8,16,18,36 Very high electrical conductivity values ranging between 2.14 × 104 and 4.1 × 104 S m−1 were also reported in some publications where only chemical agents were used for the reduction.7,27,33,46 Our results were close to these values and the addition of acetic acid into HI increased the electrical conductivity 33% when compared with the results obtained with plain HI. The worst electrical conductivity value was obtained when Hdz was used as the reducing agent. On the other hand, electrical conductivity values of GFs can reach up to 2–8 × 105 S m−1 when very high temperature thermal annealing (1300–3000 °C) reduction process was used.11,34,37 However, such thermal reductions are very costly requiring special furnaces and uses expensive inert gas atmospheres and consequently, chemical reduction is a better choice to avoid these high costs.
Some typical stress–strain curves of GFs are shown in Fig. 7. The mechanical properties of GFs after reduction were much better than that of the mechanical properties of the initial GOFs. The best tensile strength and Young's modulus values were obtained with the reduced GOF@15°-IPA sample, which was obtained in IPA bath at 15 °C as seen in Table 4. Both of the GF@25°-IPA and GF@35°-IPA samples had good tensile strength values when compared with the literature values. Tensile strength values of 8–163 MPa and Young's modulus values of 1.9–10.7 GPa were reported previously.7,16,24,36,46 It was also realized that the tensile strength values of the resultant GFs were parallel to the tensile strength values of the corresponding GOFs, similar to some reports.31,33
| Sample | Chemical reduction agent | Reduction temperature (°C) | Tensile strength (MPa) | Elongation at break (%) | Young's modulus (GPa) | Electrical conductivity (S m−1) | Reference |
|---|---|---|---|---|---|---|---|
| GF@5°-IPA | HI/AcA | 40 | 218 ± 24 | 5.7 ± 1.1 | 19.3 ± 4.0 | 1.18 ± 0.06 × 104 | This study |
| GF@15°-İPA | HI/AcA | 40 | 234 ± 26 | 5.8 ± 1.7 | 22.6 ± 4.1 | 1.28 ± 0.04 × 104 | This study |
| GF@25°-IPA | HI/AcA | 40 | 200 ± 37 | 5.7 ± 0.9 | 21.0 ± 2.7 | 1.20 ± 0.07 × 104 | This study |
| GF@35°-IPA | HI/AcA | 40 | 176 ± 33 | 5.6 ± 0.3 | 16.2 ± 3.0 | 1.19 ± 0.04 × 104 | This study |
| GF | HI (40%) | 80 | 140 | 5.8 | 7.7 | 2.50 × 104 | 7 |
| GF | HI (40%) | 80 | 182 | 3.0 | 8.7 | 0.35 × 104 | 8 |
| GF | HI (45%) | 80 | 163 ± 6 | 10.2 ± 1 | 10.7 ± 0.5 | 0.86 × 104 | 16 |
| GF | HI (45%) | 95 | 208 | 2.3 | 10.9 | 0.15 × 104 | 18 |
| GF | AsAc | 80 | 150 | 20.0 | 1.9 | 0.08 × 104 | 24 |
| GF | Thermal reduction | 220 | 115 ± 19 | 3.1 ± 0.7 | 9.0 ± 2 | 0.028 × 104 | 36 |
| GF | NaBH4 | 90 | ca. 8 | 2.8 ± 1.7 | — | 2.14 × 104 | 46 |
The best electrical conductivity value of GFs was obtained to be 1.28 × 104 S m−1 with the reduced GOF@15°-IPA sample as seen in Table 4. In general, it was determined that the effect of coagulation bath temperature on the electrical conductivities is not very important as seen in the close electrical conductivity results of the GFs samples obtained at different bath temperatures. In summary, we obtained GFs having good mechanical properties and electrical conductivities by using a coagulation bath of isopropanol at 15 °C and chemically reducing the graphene oxide filament at 40 °C using HI/AAc solution. The obtained GFs are suitable to light small bulbs (Fig. 1). It is well-known that very high tensile strength values of graphene filaments can be obtained by applying very high temperature thermal annealing to substitute carbon fiber properties.11,34,37 However, the application of high temperature thermal annealing approaching up to 3000 °C to reduce GOFs requires large investment and also consumption of large amounts of inert gases which are very expensive. Our process conditions avoid such drawbacks for the GFs, which can conduct electricity and can be used in many practical applications.
In addition, the effect of the types of the chemical reduction agents to obtain better filament electrical conductivity after reduction of GOFs at medium temperatures was investigated and it was determined that the use of hydroiodic acid/acetic acid mixture resulted in the GFs having the best electrical and also mechanical properties. The inclusion of acetic acid into hydroiodic acid increased the tensile strength 26% when compared with the plain HI treatment. It was determined that the effect of coagulation bath temperature on the electrical conductivities of final GFs was not important and the best electrical conductivity value was 1.28 × 104 S m−1 which was higher than most of the electrical conductivity results (0.03–0.86 × 104 S m−1) for the wet-spun neat GFs reported in the literature. The effect of bath temperature on the mechanical properties of final graphene filaments was very important and a tensile strength value of 234 ± 26 MPa was obtained when the bath temperature was 15 °C for an immersion duration of 2 min. This value was higher than most of the previously reported tensile strength values of GFs, which were reduced by using only chemical reducing agents at medium temperatures.
| This journal is © The Royal Society of Chemistry 2018 |