Hanan
Althikrallah
ab,
Elena F.
Kozhevnikova
a and
Ivan V.
Kozhevnikov
*a
aUniversity of Liverpool, Department of Chemistry, Liverpool L69 7ZD, UK. E-mail: kozhev@liverpool.ac.uk
bDepartment of Chemistry, King Faisal University, College of Science, P.O. Box 400, Al-Ahsa 31982, Saudi Arabia. E-mail: halhekrallh@kfu.edu.sa
First published on 14th January 2022
2,5-Dimethyltetrahydrofuran (DMTHF) is deoxygenated to n-hexane with >99% selectivity at mild conditions (90 °C, 1 bar H2 pressure, fixed-bed reactor) in the presence of the bifunctional metal-acid catalyst Pt–CsPW comprising Pt and Cs2.5H0.5PW12O40 (CsPW), an acidic Cs salt of Keggin-type heteropoly acid H3PW12O40. Addition of gold to the Pt–CsPW catalyst increases the turnover rate at Pt sites more than twofold, whereas the Au alone without Pt is not active. The enhancement of catalyst activity is attributed to PtAu alloying, which is supported by STEM-EDX and XRD analysis.
Bimetallic PtAu and PdAu catalysts have been reported to have an enhanced performance in comparison to monometallic Pt and Pd catalysts,15–31 for example, in hydrogenation,16,21,29 hydrodesulphurisation,27,28 oxidation,22,24 isomerisation15,19,30,31 and other reactions.17,18,20,25,26 The enhancement of catalyst performance by addition of gold can be attributed to geometric (ensemble) and electronic (ligand) effects of the constituent elements in PtAu and PdAu bimetallic species.25,26
Here we looked at the effect of Au on the performance of Pt–CsPW catalysts in the HDO of DMTHF in the gas phase (see the ESI for experimental details†). The CsPW heteropoly salt is a well-known solid acid catalyst; it possesses strong proton sites, large surface area and high thermal stability (∼500 °C decomposition temperature).9,32–34 Supported bimetallic catalysts PtAu/SiO2 and PtAu/CsPW were prepared by co-impregnation of H2PtCl6 and HAuCl3 onto SiO2 and CsPW followed by reduction with H2 at 250 °C (ESI†). This method gives supported bimetallic PtAu nanoparticles of a random composition together with various Pt and Au nanoparticles.15,16,31 Information about the catalysts studied is given in Table 1.
Catalyst | Surface areaa (m2 g−1) | Pore volumeb (cm3 g−1) | Pore diameterc (Å) | D d | d e (nm) |
---|---|---|---|---|---|
a BET surface area. b Single point total pore volume. c Average BET pore diameter. d Metal dispersion. e Metal particle size. f Calculated from the equation d (nm) = 0.9/D. g Metal particle diameter from powder XRD (Scherrer equation). h Pt dispersion determined by H2/O2 titration (average from three measurements); for PtAu catalysts, assumed negligible H2 adsorption on gold (see the ESI). i From STEM. | |||||
Cs2.5H0.5PW12O40 (CsPW) | 135 | 0.089 | 27 | ||
6.5% Au/SiO2 | 257 | 1.01 | 157 | 0.019f | 46g, 38i |
4.7% Au/CsPW | 103 | 0.048 | 33 | 0.016f | 60g |
6.4% Pt/SiO2 | 266 | 1.06 | 159 | 0.28 ± 0.04h | 3.2f, 8.0g, 5i |
6.0% Pt/CsPW | 84 | 0.052 | 25 | 0.17 ± 0.03h | 5.3f |
6.6% Pt/5.9% Au/SiO2 | 240 | 1.08 | 179 | 0.29 ± 0.05h | 3.1f |
5.9% Pt/4.4% Au/CsPW | 91 | 0.082 | 36 | 0.17 ± 0.04h | 5.3f |
Powder X-ray diffraction (XRD) has been widely used for the characterization of supported Au alloy catalysts.26 The XRD patterns for the silica-supported catalysts 6.4% Pt/SiO2, 6.5% Au/SiO2 and 6.6% Pt/5.9% Au/SiO2 are shown in Fig. 1. As expected, the 6.4% Pt/SiO2 and 6.5% Au/SiO2 catalysts display the fcc pattern of Pt and Au metal nanoparticles. The Pt peaks are broader than the Au peaks, which indicates a higher dispersion of Pt particles, with an average particle size of 8.0 nm for Pt and 46 nm for Au, which is in agreement with the STEM values (Table 1).
The pattern for the 6.6% Pt/5.9% Au/SiO2 catalyst clearly shows the presence of PtAu bimetallic particles with broad [111], [200], [220] and [311] diffraction peaks of the fcc PtAu alloy between the corresponding diffractions of the pure metals in the range 38–40°, 44–48°, 65–68° and 78–81°, respectively.
Fig. 2 shows the high-angle annular dark field (HAADF) STEM images of the three silica-supported catalysts 6.4% Pt/SiO2, 6.5% Au/SiO2 and 6.6% Pt/5.9% Au/SiO2 with metal nanoparticles indicated as bright spots on the darker background. In the Pt/SiO2 catalyst, there are two populations: small Pt particles of 5 nm size and coalesced Pt particles of a larger size. The Au/SiO2 catalyst displays Au particles of spherical, rectangular and triangular morphology, with an average size of 38 nm. The bimetallic PtAu/SiO2 catalyst shows a high agglomeration and different kinds of morphology of metal particles.
Fig. 2 HAADF-STEM images of (a) 6.4% Pt/SiO2, (b) 6.5% Au/SiO2 and (c) 6.6% Pt/5.9% Au/SiO2 catalysts, showing noble metal nanoparticles as bright spots. |
The energy dispersive X-ray spectroscopic analysis (EDX) of metal particles in the PtAu/SiO2 catalyst shows that these particles contain both platinum and gold. EDX elemental mapping clearly demonstrates that Pt and Au maps cover the same areas of PtAu/SiO2 catalyst (Fig. 3), indicating PtAu alloying with formation of a non-uniform bimetallic PtAu particles. More EDX mapping is presented in the ESI (Fig. S1†).
Fig. 3 HAADF-STEM image of 6.6% Pt/5.9% Au/SiO2 catalyst and the corresponding STEM-EDX elemental maps showing the spatial distribution of Au (red) and Pt (green) in the sample. |
STEM–EDX for CsPW-supported Pt, Au and PtAu catalysts has been reported elsewhere.16 These STEM images are difficult to analyse due to W, Pt and Au having similar large atomic numbers Z (74, 78, and 79, respectively). Crystalline CsPW containing 70 wt% of W displays a strong background which makes it difficult to discern smaller Pt and Au particles from the Z-contrast HAADF images and determine accurately metal particle size. Nevertheless, the STEM-EDX analysis indicates the presence of bimetallic PtAu particles in the PtAu/CsPW catalyst with a wide range of Pt/Au atomic ratios.16
Representative results for HDO of DMTHF in the presence of bifunctional metal-acid catalysts Pt–CsPW and PtAu–CsPW, which were used as physical mixtures of metal and acid components at similar Pt loadings, are shown in Table 2. The HDO reaction was carried out in flowing hydrogen at 90 °C and ambient pressure in a fixed-bed reactor (ESI†). The molar ratio of surface metal and proton sites in the catalysts was chosen low enough (Pt/H+ = 0.03–0.1) to ensure the reaction being limited by the DMTHF ring opening step.12 The density of surface Pt sites was estimated from the Pt dispersion (Table 1), the density of surface proton sites in CsPW was calculated assuming a cross section of the PW12O403− Keggin unit of 144 Å32,33 and the CsPW surface area of 135 cm2 g−1 (Table 1).
Entry | Catalyst | Conversion (%) | TOFb (h−1) | Product selectivity (% mol) | |
---|---|---|---|---|---|
n-Hexane | 2-Hexanol | ||||
a 0.20 g total catalyst weight (physical mixture of 0.020 g metal catalyst + 0.18 g CsPW), 0.6% Pt, 90 °C, 2.3 kPa DMTHF, 20 ml min−1 H2 flow rate, catalyst pre-treatment at 90 °C for 1 h in H2 flow, 1 h TOS. b TOF values per Pt surface site, the contribution of Au and CsPW subtracted. c Catalyst bed contained 0.005 g metal catalyst + 0.18 g CsPW; catalyst pre-treatment at 250 °C for 1 h in H2 flow. | |||||
1 | CsPW | 2.1 | |||
2 | 4.7% Au/CsPW + CsPW | 2.2 | |||
3 | 6.0% Pt/CsPW + CsPW | 8.6 | 70 | 98.6 | 0.7 |
4 | 5.9% Pt/4.4% Au/CsPW + CsPW | 17 | 170 | 98.6 | 0.8 |
5 | 6.5% Au/SiO2 + CsPW | 1.9 | |||
6 | 6.4% Pt/SiO2 + CsPW | 64 | 390 | 99.4 | 0.5 |
7 | 6.6% Pt/5.9% Au/SiO2 + CsPW | 85 | 490 | 99.6 | 0.3 |
8 | 6.4% Pt/SiO2 + CsPWc | 8.0 | 150 | 98.6 | 1.2 |
9 | 6.6% Pt/5.9% Au/SiO2 + CsPWc | 13 | 260 | 98.5 | 0.7 |
In the absence of Pt, the CsPW alone (entry 1) and Au–CsPW (entries 2 and 5) showed a negligible activity (1.9–2.2% DMTHF conversion with practically no 2-hexanol and n-hexane formed). Physically mixed Pt–CsPW catalysts, Pt/CsPW + CsPW and Pt/SiO2 + CsPW (1:9 w/w), exhibited a high activity giving >99% n-hexane selectivity at 8.0 to 85% DMTHF conversion depending on the catalyst and reaction conditions, in agreement with the previous report.12 It should be noted that the catalyst based on Pt/SiO2 had almost 6-fold greater activity than the one based on Pt/CsPW in terms of turnover frequency (TOF) per surface Pt site (cf. entries 3 and 6), thus demonstrating a strong effect of Pt support.
As can be seen from Table 2, the addition of gold to Pt/CsPW and Pt/SiO2 caused a significant enhancement of catalyst activity, with DMTHF conversion increasing 1.3–2 times compared to the corresponding Pt only catalysts (cf. entries 3 and 4, 6 and 7, 8 and 9). As the gold alone was practically inactive, the increase in catalyst activity can be attributed to the enhancement of activity of the Pt sites. For the bimetallic PtAu catalysts, the TOF values at Pt sites increased 1.3–2.4 times as compared to the monometallic Pt catalysts (Table 2). The results at lower DMTHF conversions of 8–17% give a more accurate estimate of the TOF enhancement reaching 1.7–2.4 times (cf. entry 3 with 4 and 8 with 9). Previously, the gold enhancement on a similar scale has been reported for alkane isomerisation on PtAu–CsPW catalysts.15,31
The enhancement of catalyst activity by addition of gold has been attributed to geometric (ensemble) and electronic (ligand) effects of the constituent metals in PtAu bimetallic nanoparticles.26 The XRD and STEM-EDX data shown above clearly demonstrate PtAu alloying in the PtAu/SiO2 catalyst leading to the formation of bimetallic PtAu species. The same has also been reported for the PtAu/CsPW catalyst.16 Previously, it has been shown that the HDO of DMTHF on Pt–CsPW is a structure-sensitive reaction,12 hence the geometric effects may be expected to contribute to the gold enhancement. However, in order to prove the role of geometric and electronic effects as the cause of the gold enhancement, more accurate metal dispersion measurements complemented by spectroscopic characterisation will be required.
We also tested the performance of bifunctional PdAu/SiO2 + CsPW and PtPd/SiO2 + CsPW bimetallic catalysts under similar conditions in comparison to the corresponding monometallic Pd and Pt catalysts. However, no enhancement of activity was observed. This is in agreement with XRD analysis, which showed no distinct PdAu alloying in PdAu/SiO2 (Fig. S2 in the ESI†).
In conclusion, we have demonstrated that the addition of gold to the Pt–CsPW catalyst has an enhancing effect on the HDO of DMTHF, increasing the turnover rate at Pt sites more than twofold. The enhancing effect is attributed to PtAu alloying. The formation of bimetallic PtAu nanoparticles in the PtAu–CsPW catalyst is confirmed by STEM-EDX and XRD.
Footnote |
† Electronic supplementary information (ESI) available: Experimental details and STEM-EDX images. See DOI: 10.1039/d1ra09105k |
This journal is © The Royal Society of Chemistry 2022 |