Youfa
Liu
a,
Qinglin
Jiang
*b,
Jiang
Zhang
b,
Wenjun
Ding
a,
Jingkun
Xu
*ac,
Peipei
Liu
a,
Guangming
Nie
c,
Haolai
Mao
a and
Fengxing
Jiang
*a
aFlexible Electronics Innovation Institute, Jiangxi Science and Technology Normal University, Nanchang 330013, P. R. China. E-mail: xujingkun1971@yeah.net; f.x.jiang@live.cn
bInstitute of Polymer Optoelectronic Materials and Devices, State Key Laboratory of Luminescent Materials and Devices, South China University of Technology, Guangzhou 510640, P. R. China. E-mail: jiangql@scut.edu.cn
cSchool of Chemistry and Molecular Engineering, Qingdao University of Science and Technology, Qingdao 266042, Shandong, P. R. China
First published on 20th June 2020
Tellurium nanowires (Te NWs) have been widely investigated in energy generators, photoelectric devices, sensors and chemical templates due to their interesting properties. However, these promising applications can be critically hindered by the inferior electrical conductivity of Te NWs and the ungreen and high energy consumption of the synthesis process. Herein, we suggest a feasible and eco-friendly strategy to synthesize Te NWs via a hydrothermal process by employing the biomolecule glucose as the reductant. The suggested strategy not only successfully avoided the use of toxic and harsh reductants and additional surfactants but also obtained Te NWs, even at low reaction temperatures. Moreover, the synthesized Te NWs presented a high electrical conductivity of 8.44 S cm−1 by optimizing the reaction conditions, and a large power factor of 97.3 μW m−1 K−2 can be obtained after annealing. Combining the variable range hopping (VRH) model with the carrier transport parameters, the PVP surfactant-weakened carrier transporting mechanism was proposed. With the as-assembled thermoelectric generator, a promising output voltage of 231 mV can be realized when the temperature difference is 80 K. The strategy shows a novel design for synthesizing highly conductive Te NWs in an eco-friendly process and presents a promising Te NWs-based thermoelectric material.
To realize the novel applications of Te NMs, a simple and feasible strategy for synthesizing Te NMs with a controllable and uniform topography in a green method is urgently required.1,17 To date, various morphologies, such as nanowires,18 nanorods,19 nanotubes,20 nanoflakes,21 and even tellurene,22 of Te NMs have been investigated, and the corresponding growth mechanisms have also been developed. For example, the solid–solution–solid growth mechanism and the nucleation–dissolution–recrystallization growth mechanism have been proposed for the generation of Te NWs23 and Te nanotubes.24 Furthermore, the intrinsically crystallography-dependent topography has also been developed, even in the absence of surfactants.25 However, most of the currently developed methods for synthesizing Te NMs are based on wet chemistry processes, where toxic reductants such as hydrazine hydrate26 or sodium borohydride27 are involved. To avoid the harms from such reductants to either humans or the environment, other mild or non-toxic reductants (ethylene glycol, ascorbic acid) have been widely utilized.28,29 Since the initially generated Te atoms in wet chemistry processes, which are so-called seeds in the reaction medium, generally tend to aggregate due to their high free energy, it is hard to present a specific topography of Te NMs under such conditions.30 Fortunately, this issue can be solved by employing surfactants such as polyvinylpyrrolidone (PVP),31 sodium dodecylbenzenesulfonate (SDBS),32 and cetyltrimethylammonium bromide (CTAB)33 as both stabilizers and templates.
Surfactants are usually employed to stabilize and induce the topography of Te NMs by adsorbing on the surface of Te NMs.34,35 However, the adsorption between surfactants and Te NMs may inevitably block the contacts between Te NMs, resulting in inferior electrical conductivity to Te NMs.15 It is also a challenge to remove the surfactants from the surface of Te NMs without undesired effects. In addition, the currently developed strategies for synthesizing Te NMs based on wet chemistry usually require high temperatures (170–200 °C),21,36 and so are risk- and energy-consuming. Recently, bacteria-assisted strategies have also been developed to synthesize Te NMs, where the bacterium is selected as the Te NMs generator in a tellurite medium.37,38 Compared with wet chemistry, this strategy successfully avoids the use of harsh reagents (toxic reductants) and surfactants, and it is safer without the additional energy input. However, it would be obstructed by the harsh survival environment of bacillus, where both the pH value and temperature of the medium would dramatically affect the survival of the bacterium. It is also time-consuming and not suitable for scale-up.
Glucose, one of the eco-friendly biomolecules, has been widely utilized to synthesize metal nanomaterials because of its reducing properties. Metal or non-metal nanomaterials, e.g., Au, Ag, Cu, Pt and Se, have been successfully synthesized by the hydrothermal process involving glucose as a reductant.39–41 On the other hand, carbonaceous nanotubes or carbonaceous Ag (Ag@C core–shell) nanocables have also been fabricated by carbonizing glucose on the surface of Te NWs or Ag NWs, and these materials can be applied in diverse fields.42–44 However, the investigation of the synthesis of Te NMs with glucose is very rare,45 and the TE performance of Te NMs obtained in such a way have also never been studied. Compared with the abovementioned strategies, glucose would be one of the most promising candidates for synthesizing Te NMs due to the following advantages. (1) Glucose is a green reductant, eco-friendly and bio-friendly. (2) It is renewable, easy-to-get and low-cost. (3) Apart from acting as a reductant, glucose can also act as a surfactant in the hydrothermal process. (4) Due to the good water-solubility of glucose, the re-dispersibility of Te NMs would be considerable when glucose is employed as a reductant. (5) No high temperature is needed due to the reduction of the aldehyde group.
In this work, we developed a simple and eco-friendly strategy to synthesize Te NWs by utilizing the biomolecule glucose as the reductant. Herein, no toxic reductant and additional surfactant were involved, and the reaction conditions were also systematically investigated. With the synthesized Te NWs, thin pieces were fabricated by combining the vacuum filtration and pressing process, and their TE performances were also systematically studied by varying the reaction and annealing conditions. To understand the high electrical conductivity of the as-fabricated Te NWs thin pieces, the one-dimensional variable range hopping (VRH) model was fitted based on the temperature-dependent electrical conductivity. Furthermore, a simple TEG with 10 pieces of the as-fabricated Te NWs thin pieces was assembled, and the output performance was measured at the temperature difference from 0 to 80 K. Finally, the air-stable TE performance of the as-fabricated Te NWs thin piece was illustrated by investigating the time-dependence of the TE performance. This work will provide a green and feasible method for synthesizing highly conductive Te NWs and develop a new strategy to design a promising Te NWs-based TE material.
To design the TE generator, the as-fabricated Te NWs thin piece was cut into rectangles (13.0 × 2.00 mm2) and 10 of the rectangles were connected in series by copper wires and silver paste (as shown in Fig. 6A). The output performance of the as-fabricated TE generator was evaluated by building a temperature difference (ΔT) at the two ends of the rectangles at room temperature.
2CH2OH–(CHOH)4–CHO + TeO32− → 2CH2OH–(CHOH)4–COO− + Te + H2O. |
Fig. 1 Schematic illustration of the synthesis of Te NWs with glucose as the reductant, and the fabrication of Te NWs thin pieces. |
XPS spectra (Fig. 2A) and XRD patterns (Fig. 2B) were obtained to verify the generation of Te NWs and their phase structure. As seen in Fig. 2A, the Te NWs synthesized with glucose at 120 °C for 12 h presented two typical Te3d3/2 and Te3d5/2 peaks,48 suggesting that glucose can act as the reductant to synthesize Te. To optimize the reaction conditions for synthesizing Te NWs, the reaction temperature (from 60 to 180 °C) and reaction time (from 10 to 20 h) were varied. Fig. 2B shows the XRD patterns of Te NWs synthesized at 90, 120, 150 °C for 12 h, while the Te NWs were synthesized at 180 °C for 12 h; the N2H4·H2O-synthesized Te NWs are presented in Fig. S1 (ESI†). As shown in Fig. 2B, the Te NWs synthesized with glucose presented identical diffraction peaks, which can be indexed to the standard card (JCPDS# 36-1452) of tellurium with a hexagonal phase.31 The results from the XRD patterns further indicate that Te can be synthesized with glucose as the reductant, even if the hydrothermal temperature was as low as 60 °C. Compared with other methods,49,50 Te can be easily synthesized in this work with no toxic and harsh reagents and no high temperature involved, suggesting that this strategy is more green and is feasible for synthesizing Te NMs.
Fig. 2C–E displays the SEM images of the Te NWs synthesized with glucose at 90 °C (C), 120 °C (D) and 150 °C (E) for 12 h; the Te NWs synthesized with N2H4·H2O are presented in Fig. S2 (ESI†). As can be seen, all Te NWs had a nanowire morphology, which can be ascribed to the anisotropy of Te NWs along its c-axis.16 Due to the strong polarity and the long chain of PVP, it can effectively control the nucleation and growth of Te NWs due to the template effect and steric effect as reported in previous works.32,51 Therefore, the Te NWs synthesized with N2H4·H2O were significantly thinner and longer as compared to the glucose-synthesized Te NWs. Notably, the Te NWs can be synthesized in this work even in the absence of surfactant, which can be attributed to the surfactant effect of glucose. Similarly, there are many previous reports in which glucose was utilized as a surfactant to synthesize nanomaterials.52–54 To further illustrate that glucose can act as a surfactant in this work, C element was detected in the Te NWs synthesized with glucose at 120 °C for 12 h by EDS spectroscopy (Table S1, ESI†), where C arose from glucose being adsorbed on the surface of Te NWs. Based on the dual-role of glucose, the glucose-assisted self-assembly mechanism was proposed for the synthesis of Te NWs. Firstly, sodium tellurite was reduced to the Te nuclei by glucose in the solution. After that, with the assistance of the glucose surfactant, these fresh Te nuclei would prefer to assemble on the glucose surfactant to minimize their free energy. The Te nuclei adsorbed on the glucose surfactant would act as crystal seeds to adsorb Te atoms from solution to form the larger Te nuclei. Finally, the generated Te atoms in the solution would continuously adsorb onto their vicinal mature Te nuclei and grow along its c-axis, due to the inherently anisotropic property of trigonal Te. Therefore, Te NWs can be generated with the consumption of Te in the solution. Fig. 2F shows the photo of the as-fabricated Te NWs thin piece after pressing under 15 MPa for 15 min, revealing the dense and smooth property of the pressed materials.
Samples | n (1018 cm−3) | μ (cm2 V−1 s−1) | σ (S cm−1) | σS 2 (μW m−1 K−2) | Ref. |
---|---|---|---|---|---|
a The Te NWs were synthesized with glucose at 120 °C for 12 h and without annealing. b The Te NWs were synthesized with N2H4·H2O and without annealing. c The Te NWs were synthesized with glucose at 120 °C for 12 h and this as-fabricated Te NWs thin piece was annealing at 350 °C for 3 h. d The Te NWs were synthesized with N2H4·H2O and this as-fabricated Te NWs thin piece was annealing at 350 °C for 3 h. | |||||
Te NWs | 0.017 | 33.7 | 0.08 | 3.61 | 56 |
Te NPs | 0.135 | 2.95 | 0.22 | — | 58 |
Te NWs | 2.01 | 0.46 | 0.04 | 1.25 | 55 |
Te NWs | — | — | 0.005 | 0.11 | 15 |
Te NRs | — | — | 0.1 | 1.6 | 57 |
Te NWsa | 3.83 | 13.8 | 8.44 | 67.5 | This work |
Te NWsb | 1.12 | 2.4 | 0.42 | 8.2 | |
Te NWsc | 4.17 | 11.5 | 7.68 | 97.3 | |
Te NWsd | 0.17 | 65.5 | 7.44 | 99.7 |
To further improve the TE performance of the optimized Te NWs thin pieces, they were annealed under different conditions. Fig. 3E and F shows the TE performance of these optimized Te NWs thin pieces after annealing; the TE performance of the N2H4·H2O-synthesized Te NWs after annealing are presented in Fig. S3 (ESI†). As observed in Fig. 3E, the electrical conductivity of the optimized Te NWs thin pieces increased with the increasing annealing temperature, but a further increase in temperature led to decreased electrical conductivity. However, the maximum electrical conductivity (7.68 S cm−1) of the annealed Te NWs thin pieces was lower than that of the unannealed pieces (8.44 S cm−1), which may result from the thin pieces being relatively less dense after annealing, where the density of the optimized Te NWs thin pieces decreased from 2.4 to 2.2 g cm−3 after annealing. The S value of the annealed Te NWs thin pieces was improved to 356.8 μV K−1 after annealing at 450 °C for 3 h, and an enhanced power factor of 97.3 μW m−1 K−2 was achieved on annealing at 350 °C for 3 h. The enhanced value is significantly higher as compared to the previous works as listed in Table 1. In addition, we varied the annealing time from 0 to 3 h at the optimized annealing temperature of 350 °C. As shown in Fig. 3F, the electrical conductivity was slightly increased and then decreased with increasing annealing time. The Seebeck coefficient was increased monotonically, and the maximum power factor was reached at 350 °C for 3 h. It is worth noting that the TE performance of the Te NWs synthesized with N2H4·H2O was greatly enhanced due to the improved electrical conductivity (7.44 S cm−1) in Fig. S3 (ESI†), and a large power factor of 99.7 μW m−1 K−2 was obtained on annealing at 350 °C for 3 h. According to the previous work,56 this greatly improved electrical conductivity can be ascribed to the carbonization of PVP during the annealing process, thus greatly enhancing the power factor.
To understand the effects of annealing on the TE performance of the optimized Te NWs thin pieces, the XRD patterns (Fig, S4, ESI†) and EDS spectrum for elemental analysis (Table S1, ESI†) were obtained for these optimized Te NWs thin pieces with or without annealing. As observed in Fig. S4 (ESI†), the Te NWs thin pieces after annealing showed the same diffraction peaks as hexagonal tellurium (JCPDS# 36-1452). It should be noted that as the annealing temperature increased to 350 °C, the intensity of the 100 and 110 peaks changed significantly and the 100 peak became much stronger. This indicates that the increase in annealing temperature led to a decrease in the diameter of Te NWs.59 Interestingly, the further increase in annealing temperature to 450 and 550 °C resulted in the intensity of the 100 peak being weakened again, suggesting the increase in the diameter of Te NWs. This revealed that the melting point of Te NWs was about 450 °C. The further increase in the annealing temperature to 550 °C caused the re-aggregation of Te NWs and the larger diameter. Moreover, the crystallinity shown in Table S1 (ESI†) changed with the increase in the annealing temperature. Increased crystallinity was observed for Te NWs thin pieces annealed at lower temperatures than 450 °C. This increase in crystallinity would be beneficial for electrical conductivity. On the other hand, the C element content and the atom ratio of C/O for these thin pieces annealed at temperatures lower than 450 °C were slightly changed, indicating no carbonization of glucose for these Te NWs thin pieces.60 However, they were obviously increased when the annealing temperature was higher than 350 °C, due to the carbonization of glucose and evaporation of Te atoms at high temperature. Therefore, as shown in Fig. 3E, the electrical conductivity of the optimized Te NWs thin pieces was decreased for a further increase in the annealing temperature, leading to the decreased TE performance at high temperature.
As mentioned above, the biomolecule glucose not only acts as a reductant, but can also act as a surfactant to assist in synthesizing Te NWs with promising electrical conductivity as compared to that synthesized with N2H4·H2O. Based on the surfactant role of PVP and glucose, a schematic illustration is proposed in Fig. 4A to understand the high electrical conductivity of the glucose-synthesized Te NWs. Since PVP is a polymer with strong polarity and a long chain, it can strongly adsorb on the surface of Te NWs to induce the nucleation and growth of Te NWs during the hydrothermal process, resulting in PVP-wrapped Te NWs. Simultaneously, some carbonaceous molecules resulting from the carbonization of PVP will also be adsorbed on the surface of Te NWs. However, the adsorption of PVP and carbonaceous molecules on the surface of Te NWs would critically block the contacts between Te NWs, which hinders the hopping of carriers among Te NWs. In addition, the presence of PVP and carbonaceous molecules may enhance the hopping barrier energy for carriers. Therefore, carriers with low energy would be greatly scattered at the interface between Te NWs, thus causing the inferior electrical conductivity of Te NWs. In contrast, as stated in Fig. 4A and Fig. S5 (ESI†), there are only small carbonaceous molecules adsorbed on the surface of the glucose-synthesized Te NWs. Carriers can easily transport to the nearby Te NWs, resulting the high electrical conductivity of the glucose-synthesized Te NWs. In addition, as shown in Fig. 1, a pressing process was employed to fabricate the Te NWs thin pieces. The pressing process can result in a dense thin piece, which enhances the contact between Te NWs and enables the high electrical conductivity.
To illustrate the conductive properties and describe the high electrical conductivity of the glucose-synthesized Te NWs, the temperature-dependent electrical conductivity of the optimized Te NWs thin pieces and the N2H4·H2O-synthesized Te NWs before (Fig. 4B) and after (Fig. S6A, ESI†) annealing at 350 °C for 3 h are presented. As seen in Fig. 4B, the electrical conductivity of the Te NWs thin pieces decreased with decreasing temperature for both glucose and N2H4·H2O-synthesized Te NWs, indicating typical semiconductor behavior.58 To reveal the high electrical conductivity of Te NWs synthesized with glucose, we fitted the temperature-dependent conductivity of these Te NWs thin pieces before and after annealing with the 1D variable range hopping (VRH) model in Fig. 4C and Fig. S6B (ESI†). In the above formula, σ0 and T0 are the constants, the characteristic temperature related to the energy barrier constant for the hopping of carriers from nanowire to nanowire, and d is the dimensionality of the conducting material (herein, the d is 1).56 In this work, the estimated T0 values for the Te NWs synthesized with glucose and N2H4·H2O before annealing are 35 and 56 K, respectively. The much lower T0 for glucose-synthesized Te NWs can be used to illustrate the PVP surfactant-hindered transport properties, where the hopping of carriers was blocked and the high hopping barrier energy for carriers due to the strong wrapping of PVP on the surface of Te NWs. Therefore, the electrical conductivity of the glucose-synthesized Te NWs was significantly higher than that synthesized with N2H4·H2O. Furthermore, after annealing at 350 °C for 3 h, not only was the T0 value greatly decreased to 20 K, but also the electrical conductivity was dramatically enhanced to 7.44 S cm−1 for N2H4·H2O-synthesized Te NWs, which may be attributed to the degradation and carbonization of PVP during the annealing process. This can be further used to understand the hindered carriers by PVP and the high electrical conductivity of glucose-synthesized Te NWs. To fully reveal the high electrical conductivity of the glucose-synthesized Te NWs, we studied the transport parameters of both carrier concentration (n) and mobility (μ) of the optimized Te NWs thin pieces and N2H4·H2O-synthesized Te NWs before and after annealing at 350 °C for 3 h. Fig. 5 shows the Hall resistance value of these Te NWs thin pieces as a function of the magnetic field. According to the relationship between the Hall resistance and magnetic field, the n and μ of these Te NWs thin pieces can be obtained. As listed in Table 1, both the n and μ value of the glucose-synthesized Te NWs are much higher than that of the N2H4·H2O-synthesized Te NWs or previously reported NWs, suggesting that the presence of PVP on the surface of Te NWs may obstruct and scatter the carriers with low energy. Therefore, the glucose-synthesized Te NWs can present much higher electrical conductivity due to the larger n and μ based on σ = μne. Apart from investigating the electrical conductivity of the optimized Te NWs thin pieces with or without annealing at 350 °C for 3 h at low temperature, the temperature-dependent Seebeck coefficient of these Te NWs thin pieces was also studied as shown in Fig. S7 (ESI†). A decreased S value was observed for these Te NWs thin pieces with or without annealing. Therefore, decreased TE performance was observed in low-temperature conditions.
To assess the output performance of the optimized Te NWs thin pieces, we assembled a TEG prototype with 10 pieces of the optimized Te NWs thin pieces (13.0 × 2.0 × 0.052 mm3) as TE legs. As displayed in Fig. 6A, all the TE legs were connected by copper wire in series. The output voltage of the TEG versus the temperature difference was recorded as shown in Fig. 6B (black line). The output voltage was evenly increased with an increasing temperature difference (ΔT) from 0 to 80 K. The slope of the fitted line (red line in Fig. 6B) between the output voltage and ΔT was 2881 μV K−1, which is similar to the total Stol value of the as-assembled TEG based on the formula: Vtol = n × (Sp − Sn) × ΔT, where n, Sp, Sn are, respectively, the number of the p or n-type TE leg, and the Seebeck coefficients of the p and n-type TE legs. In our work, no n-type TE legs were employed; therefore, the value of n is 10, and the Sp of the optimized Te NWs thin piece was measured as 282.5 μV K−1 above. The inset in Fig. 6B is the schematic illustration for the measurement of the S value. The output voltage can be up to 111 mV at ΔT of 40 K, and this value would be further improved to 231 mV with ΔT of 80 K. The output performance of our assembled TEG is one order of magnitude higher than that of the Te NMs-based TEG, even though no n-type TE legs were employed in this work,16,57,61,62 which is more promising for energy harvesting.
Finally, we investigated the air-stable TE performance of the optimized Te NWs thin pieces versus the time in ambient conditions, which are presented in Fig. S8 (ESI†). As displayed, the electrical conductivity, Seebeck coefficient or power factor of the optimized Te NWs thin pieces synthesized with glucose or N2H4·H2O degenerated with the extended time. For the Te NWs synthesized with glucose, the power factor was only decreased by 2% as compared with the original value when the fresh Te NWs thin pieces were kept at ambient conditions for 5 days, and it continuously decreased to 45% over 30 days. However, the power factor of the N2H4·H2O-synthesized Te NWs was decreased from 80 to 28% when the time was extended from 5 to 30 days. The significantly decreased power factor for the N2H4·H2O-synthesized Te NWs suggests that the glucose-synthesized Te NWs presented a more air-stable TE performance. To verify the more air-stable TE performance of the glucose-synthesized Te NWs, the C1s (Fig. S5, ESI†) and Te3d (Fig. 2 and Fig. S9, ESI†) XPS spectra of the Te NWs synthesized with glucose and N2H4·H2O (both the fresh NWs and those stored under ambient conditions for 30 days) were recorded. As observed in the Te3d XPS spectra, the Te3d5/2 (Te4+) and Te3d3/2 (Te0) peaks were present in all Te NWs samples. Notably, the integral ratio of Te3d5/2 (Te4+) to Te3d3/2 (Te0) was increased with extending the time for both glucose and N2H4·H2O-synthesized Te NWs, but the increased value for the N2H4·H2O-synthesized Te NWs was dramatically higher than that of the glucose-synthesized one, suggesting that the N2H4·H2O synthesized Te NWs are easier to oxidize under ambient conditions.48 In addition, as seen in Fig. S5 (ESI†), a stronger and wider C1s peak was observed for the glucose-synthesized Te NWs, illustrating that the presence of carbonaceous molecules on the surface of Te NWs would more effectively prevent Te NWs from being oxidized. Therefore, the glucose-synthesized Te NWs are more stable under ambient conditions and demonstrate the more air-stable TE performance.63
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d0ma00220h |
This journal is © The Royal Society of Chemistry 2020 |