aEngineering Research Center of High-frequency Soft Magnetic Materials and Ceramic Powder Materials of Anhui Province, Chaohu University, 1 Bantang Road Chaohu, Hefei, 238024, P. R. China. E-mail: little_weihui@yahoo.co.jp; 053063@chu.edu.cn
bBaoji Oilfield Machinery Co., Ltd, Baoji, 721002, P. R. China
cHefei Jingchuang Technology Co., Ltd, Hefei, 231500, P. R. China
First published on 29th January 2024
We have devised a moderate temperature spark plasma sintering route for preparing aluminum matrix composites which possess tailored coefficients of thermal expansion (CTEs) in combination with tunable electrical and thermal conductivities. Due to its isotropic negative thermal expansion over a wide temperature range, cubic-phase ZrW2−xMoxO8 (x = 0.0, 1.0) is an ideal secondary phase for metal matrix composites with suitable CTEs. In this study, high-density ZrW2O8/Al and ZrWMoO8/Al composites containing 30–70 vol% Al were fabricated using spark plasma sintering. X-ray diffraction analysis indicated that the composites were composed of a thermally-stable cubic phase at temperatures as high as 873 K for ZrW2O8 and 773 K for ZrWMoO8, without any orthorhombic high-pressure phase derived from the large thermal mismatch between the ceramic and metal during sintering. The thermal expansion curves of the ZrW2−xMoxO8/Al composites were consistent with the predictions made using the Rule-of-Mixtures. The CTEs could be controlled from negative to positive and even close to zero by simply varying the volume fraction of aluminum. Similarly, the thermal and electrical conductivity of the ZrW2−xMoxO8/Al composites increases with increasing Al content, which is thought to be mainly related to the contribution of the free electron conduction path of Al in the composites.
Cubic-phase ZrW2O8 is a typical material with a negative thermal expansion, which demonstrates a large three-dimensional isotropic NTE coefficient (−8.8 to −4.9 × 10−6 K−1) over a wide temperature range (0.3–1050 K).4–7 These characteristics render it an ideal secondary phase for aluminum matrix composites with suitable thermal expansion coefficients. Near 443 K, ZrW2O8 undergoes a reversible order–disorder phase transition from a low-temperature acentric cubic phase (α-ZrW2O8: −8.8 × 10−6 K−1) to a high-temperature centric cubic phase (β-ZrW2O8: −4.9 × 10−6 K−1).6–8 The abrupt change of NTE coefficient is a disadvantage in practical applications if the phase transition temperature of the materials is within the working temperature range. Numerous investigations have confirmed that the phase transition temperature of ZrW2O8 can be adjusted through Mo6+ partially doping in W6+, which it was reported that increasing the Mo content in ZrW2−xMoxO8 leads to a lower phase transition temperature.9–13 J. S. O. Evans et al.10 reported that the α–β phase transition temperature shifted to below room temperature for ZrWMoO8 by conducting neutron powder diffraction experiments, indicating that ZrWMoO8 is also a very promising inhibitor of thermal expansion. However, due to its relatively modest thermal expansion coefficient above room temperature (−3.5 × 10−6 K−1), its applicability to composite materials is somewhat limited. Therefore, comparing the thermal expansion properties of composites by incorporating ZrW2O8 and ZrWMoO8 separately as thermal expansion inhibitors with Al is crucial for practical applications.
In addition, low-temperature cubic phase α-ZrW2O8 transforms into an orthorhombic phase (γ-ZrW2O8), when subjected to pressures above 0.2 GPa, with a dramatically low NTE coefficient, which decreases from −8.8 to −1.0 × 10−6 K−1.14–16 It has been reported that γ-ZrW2O8 was formed during ZrW2O8/Al composite sintering, wherein the cubic–orthorhombic phase transition strongly influenced the thermal properties of the composites, due to the different thermal expansion coefficients of the ceramic and metal matrix particles.1,17,18 Similar phenomena were also observed in other metal matrix composites containing ZrW2O8 particles such as ZrW2O8/Cu, ZrW2O8/Al–Si composites.19–24 The biggest disadvantage of ZrW2O8/Al composites is their high sintering temperature, which causes ZrW2O8 to decompose into ZrO2 and WO3 above 1050 K, whereas the melting point of aluminum is about 933 K.25 Therefore, a low-temperature, low-pressure sintering method is needed for the fabrication of ZrW2−xMoxO8/Al composites in order to suppress the α–γ phase transition.
Spark plasma sintering (SPS) is a promising method for bonding various kinds of solid materials (e.g., metal to metal, metal-to-ceramic, etc.). The mechanism of SPS involves the instantaneous generation of high-temperature spark plasma in the gap due to the discharge effect between the powder particles. Throughout the SPS process, the combined effects of spark discharge (leading to the generation of spark plasma and localized spark impact pressure), Joule heating, electrodiffusion, and plastic deformation contribute to fast and efficient sintering. Our group synthesized single-phase ZrW2O8 ceramics and ZrW2O8/SiO2 and ZrW2O8/Cu composites at 873 K and 50 MPa by using SPS.26,27 Since the melting point of aluminum is about 933 K, this coincides well with the synthesis temperature of ZrW2O8 in our past work, which facilitates a better synergy between the two materials in the composite process. In this study, dense ZrW2−xMoxO8/Al (x = 0.0, 1.0) composites containing 30 to 70 vol% Al were fabricated using SPS. We investigated the effects of ZrW2−xMoxO8 as thermal expansion inhibitors on the thermal expansion properties of the composites and carried out a comparison of the thermal expansion curves with predictions made using the Rule-of-Mixtures. In addition, the thermal conductivity and electrical conductivity of the ZrW2−xMoxO8/Al composites were evaluated to explore the application prospects of the composites.
The second stage is referred to as the hydrothermal stage. The obtained sol–gel precursors were dissolved in 60 mL of distilled water and after addition to a 100 mL Teflon-lined Parr bomb, placed in a mantle heater at 453 K for 18 hours with continuous stirring. The sol–gel-hydrothermal precursors were finally centrifuged, washed with distilled H2O, and dried in an oven at 333 K. The sol–gel-hydrothermal precursors were pre-calcined at 873 K for ZrW2O8 in a drying oven (DX-41, Yamato Scientific, Tokyo, Japan). Aluminum powders (Kojundo Chemical, 99.99%, Tokyo, Japan) were mixed with ZrW2O8 and ZrWMoO8 powders at various volume ratios (0 vol% Al, 30 vol% Al, 50 vol% Al, 70 vol% Al, 100 vol% Al). Ethanol was added to the mixed powders, and the mixture was kneaded for 30 min in an agate mortar. After kneading, the mixed powders were placed in a drying oven at 373 K for 3 h. The mixed powders were filled in graphite dies (10 mm in diameter and 20 mm in depth) separately and wrapped in carbon sheets. An SPS apparatus (SPS-515S; Fuji Electronic Industrial, Saitama, Japan), with a pulse duration of 3.3 ms and on/off pulse intervals of 12
:
2, was used to fabricate dense ZrW2O8/Al and ZrWMoO8/Al composites. The composites were sintered at 873 K (ZrW2O8/Al) and 773 K (ZrWMoO8/Al) for 10 min at a heating rate of 100 K min−1 to obtain ZrW2−xMoxO8/Al composites. During SPS, the applied pressure was held constant at 90 MPa in an argon atmosphere, until the conclusion of the sintering process. The volume contraction between the two graphite punches, namely the Z-axis linear shrinkage value, was recorded every 30 s during SPS. The Z-axis linear shrinkage curve of Al 50 vol% ZrW2O8/Al composite and optical photos of ZrW2O8/Al composites with different Al volume fractions are shown in Fig. 1.
![]() | ||
| Fig. 1 Z-axis linear shrinkage curve of Al 50 vol% ZrW2O8/Al composite and optical photos of ZrW2O8/Al composites. | ||
100 nA. The coefficients of thermal expansion of the samples were measured with a thermodynamic analyzer (Shimadzu, TMA-60/60H, Kyoto, Japan). The data were collected at a heating rate of 1 K min−1 from 323 to 523 K and three replicate experiments were carried out. The theoretical CTEs of the composites were calculated using the Rule-of-Mixtures. The Rule of Mixtures (ROM) is a theoretical framework used to predict the properties of composite materials based on the volume fractions and properties of the individual components. ROM considers the matrix to be free of voids, in which each material is perfectly bonding to the matrix so that each component is distorted independently. Coefficients of thermal expansion are usually assumed to follow a linear ROM dependence on the volume fraction. The CTE values used were as follows: 23 × 10−6 K−1 for Al, −8.8 × 10−6 K−1 for low-temperature cubic phase α-ZrW2O8, −4.9 × 10−6 K−1 for high-temperature cubic phase β-ZrW2O8, and −3.5 × 10−6 K−1 for ZrWMoO8.29 The relative densities of the composites were measured by Archimedes' principle using distilled water. The specific Archimedes method steps are as follows: obtain post-sintered samples of ZrW2O8/Al and ZrWMoO8/Al composite materials, ensuring that their surfaces are clean and free of impurities. Then, use a precision balance to weigh the mass of each sample and record the accurate mass values (m1). Subsequently, gently and uniformly immerse the samples in deionized water, ensuring that no bubbles adhere to the sample surfaces. Wait for stability and record the mass of the samples when submerged in deionized water (m2). Calculate the relative density (ρr) using the following formula: ρr = m1/[(m1 − m2) × ρl], where ρl is the density of deionized water at ambient temperature. The measured density of all specimens as well as the theoretical values have been listed in Table 1. The theoretical densities of the composites were calculated by using reference data (the density of Al is 2.70 g cm−3) based on the theoretical density of α-ZrW2O8 (ρ = 5.08 g cm−3).6 The measured density of all specimens exceeded 90% of the theoretical value, and that of the ZrW2−xMoxO8/Al (x = 0.0, 1.0) specimens were close to the estimated theoretical density. Furthermore, the relative density of the ceramic–metal composites was found to increase with the increase in metal content. The coefficients of thermal diffusion and the specific heat were measured by the conventional laser flash method using a thermal constant analyzer (ULVAC, TC7000, Kanagawa, Japan). The thermal conductivity coefficients were calculated from the experimental thermal diffusivity as well as the specific heat capacity and density values, which were measured by Archimedes' principle.
| Al volume fraction (vol%) | ZrW2O8/Al | ZrWMoO8/Al | ||||
|---|---|---|---|---|---|---|
| Density (g cm−3) | Theoretical density (g cm−3) | Relative density (%) | Density (g cm−3) | Theoretical density (g cm−3) | Relative density (%) | |
| 0 | 4.80 | 5.08 | 94.5 | 4.17 | 4.33 | 96.3 |
| 30 | 4.10 | 4.37 | 93.8 | 3.56 | 3.84 | 92.7 |
| 50 | 3.91 | 3.89 | 101 | 3.33 | 3.52 | 93.9 |
| 70 | 3.35 | 3.41 | 98.2 | 2.93 | 3.19 | 91.9 |
| 100 | 2.69 | 2.70 | 99.8 | 2.69 | 2.70 | 99.8 |
). The fabrication stress during SPS and the thermal stress between ZrW2O8 and Al was not high enough to be able to induce cubic–orthorhombic phase transition, which suggests the successful fabrication of ZrW2O8/Al composites without a high-pressure phase transition. However, some Al2O3 characteristic reflections were observed due to the partial oxidation of aluminum. Fig. 2(c) and (d) correspond to the (012) and (112) reflections in Fig. 2(a) and (b), respectively. No clear reflection shift was observed in the XRD patterns of the ZrWMoO8/Al specimens, whereas the reflections of ZrW2O8/Al specimens shifted to higher angles as the Al volume fraction. In addition, the full width at half maximum (FWHM) of ZrW2O8/Al specimens increased upon increasing the Al volume fraction. This may be due to the fact that at lower sintering temperatures, ZrWMoO8 has a relatively smaller compressive strain in the aluminum matrix than ZrW2O8 grains, and this difference in compressive strain will be reflected in the thermal expansion results below. The crystallite size corresponding to the FWHM of certain reflections (012, 112) using the Scherrer formula was calculated. The crystallite size range for the ZrW2O8/Al sample is between 120 nm and 180 nm, while for the ZrWMoO8/Al sample, it falls between 170 nm and 270 nm. A comparison reveals that the crystallites in the ZrW2O8/Al specimens are finer than those in the ZrWMoO8/Al specimens.
Fig. 3(a)–(f) shows the backscattered electron images of the microstructure of the polished surface of ZrW2−xMoxO8/Al (x = 0.0, 1.0). Different ceramic compositions resulted in different homogeneity of composites. Especially in the Al 70 vol% ZrW2−xMoxO8/Al composites, many 1 μm to 10 μm aggregates were observed in the ZrW2O8/Al specimen, whereas in the ZrWMoO8/Al specimen, the aggregates had sizes from 100 nm to 1 μm, and the homogeneity of Al and ZrWMoO8 was improved. The dispersed particles were smaller in the ZrWMoO8/Al specimens, and there was less particle agglomeration. As a result, because the specific surface area of ZrW2O8 particles was larger than Al, the compressive stress generated from Al during cooling is expected to be larger than that in the ZrWMoO8/Al specimens.
![]() | ||
| Fig. 3 (a–f) SEM images of the polished surface of ZrW2−xMoxO8/Al (x = 0.0, 1.0) composites; (g) SEM-EDX point analysis of the Al 30 vol% ZrW2O8/Al specimen. | ||
To better understand the dispersion of Al and ZrW2O8 particles and the composition of each component of the composites, SEM-EDX point analysis was employed for investigating the elemental composition at six points of Al 30 vol% ZrW2O8/Al specimen (Fig. 3(g)). Point 1 seems to have ZrW2O8 as the main phase because the quantitative analysis shows that the ratio of Zr
:
W is about 1
:
2. Point 2 seems to have Al as the main phase, and the existence of oxygen may be related to the oxidation of Al, but oxygen doesn't exist in a significant quantity. Al was highly oxidized at Point 4, which presumably lies near the tissue interface of Al and ZrW2O8. This is inevitable because the oxide-forming tendency of Al is low in comparison with other metals. The sparse black spots (Point 3 and Point 5) in the SEM image have a Zr
:
W ratio that deviates from 1
:
2. These spots may be due to impurities such as Al2O3 that were introduced as contaminants at the time of powder production. The same applies to Point 6.
Fig. 4(c) and (d) depicts the changes in the CTEs after the heating cycle relative to the volume fraction of Al. In ZrW2O8/Al specimens, a convex parabolic trend can be observed, with the maximum CTE reached at 50 vol% Al. The change in the CTEs of ZrW2O8/Al specimens was about 0.1 to 0.3%, whereas the CTE variation of the ZrWMoO8/Al sample remains more or less constant. This difference in CTE seems to be related to the dispersion state of ZrW2−xMoxO8 with Al. In the ZrW2O8/Al specimens, because the ZrW2O8 particles formed 100 μm agglomerates, the stress from Al relieved the agglomeration and pores of ZrW2O8. The ZrW2O8 particles subjected to stress from Al increased because the dispersed particle size was small in the ZrWMoO8/Al specimens.
The thermal expansion behavior of the composites was further analyzed by comparing the experimental results with theoretical models. Several models have been proposed to estimate the CTEs of ceramic–metal composites.30–32 Among them, the most widely used is the (ROM). ROM considers the matrix to be free of voids, in which each material is perfectly bonding to the matrix so that each component is distorted independently. CTEs are usually assumed to follow a linear ROM dependence on the volume fraction. Fig. 5(a) and (b) shows the thermal expansion of ZrW2−xMoxO8/Al (x = 0.0, 1.0) composites with different Al volume fractions obtained from the third heating cycle and a comparison with the values predicted by the ROM model. In contrast to the measured curves of ZrWMoO8/Al composites were consistent with the theoretical curves of the ROM model, the measured curves of ZrW2O8/Al composites show a slight deviate from the theoretical curves of the ROM model, possibly due to the presence of nanoparticles, which led to residual stresses in the composites. Furthermore, the thermal expansion behavior of both composites confirmed that the CTEs changed from negative to near-zero to positive by changing the volume fraction of Al. For ZrW2O8/Al composites, mon-linear changes in the CTEs were observed around 420–440 K, which was associated with the order–disorder phase transition of α-ZrW2O8 to β-ZrW2O8.
![]() | ||
| Fig. 5 TMA curves of (a) ZrW2O8/Al and (b) ZrWMoO8/Al composites during the third heating cycle; CTEs of (c) ZrW2O8/Al and (d) ZrWMoO8/Al composites. | ||
The CTEs of ZrW2−xMoxO8/Al (x = 0.0, 1.0) composites measured by thermo-mechanical analysis and estimated based on the ROM model are plotted in Fig. 5(c) and (d). The measured coefficients have values similar to the values reported for ZrW2O8 powders in the literature (α-ZrW2O8: −8.8 × 10−6 K−1; β-ZrW2O8: −4.9 × 10−6 K−1). Compared with the ZrW2O8/Al composites, the ZrWMoO8/Al composites had slightly higher CTEs because the absolute value of the negative CTEs value of ZrWMoO8 is smaller than that of ZrW2O8. Additionally, when the Al content rises, the value of the CTEs of ZrW2O8/Al composites at the room temperature gradually increases, from −8.46 × 10−6 K−1 for ZrW2O8 to 3.37 × 10−6 K−1 for Al 30 vol% specimen, 11.90 × 10−6 K−1 for Al 50 vol% specimen and rised to 17.20 × 10−6 K−1 for Al 70 vol% specimen. The same phenomenon was observed in ZrWMoO8/Al composites, where the CTEs increased from −3.49 × 10−6 K−1 for ZrWMoO8 to 10.54 × 10−6 K−1 for Al 30 vol% specimen, 17.29 × 10−6 K−1 for Al 50 vol% specimen, and 20.00 × 10−6 K−1 for Al 70 vol% specimen. This indicates that ZrW2−xMoxO8/Al (x = 0.0, 1.0) composites with a tunable thermal expansion coefficient (negative, positive, or close to zero) could be produced by adjusting the volume fraction of Al. Thus, this result suggests that the CTEs can be controlled to some extent by using ZrWMoO8 as an inhibitor, as in the case of ZrW2O8. The two NTE ceramic materials as inhibitors have their own characteristics in controlling the thermal expansion properties, among which ZrW2O8 has a larger NTE coefficient, which can maintain the original properties (such as electrical conductivity, thermal conductivity) of the composite matrix, to a greater extent while regulating the CTEs; on the other hand, the advantage of ZrWMoO8 is that it does not have the phase transition from the low-temperature phase to the high-temperature phase above room temperature, which avoids the drastic change of the CTEs during phase transition.
![]() | ||
| Fig. 6 (a) Thermal conductivity and (b) electrical conductivity of ZrW2−xMoxO8/Al composites at room temperature. | ||
![]() | ||
| Fig. 7 Simulation diagram of internal electron conduction in ZrW2O8/Al composites with different Al volume fraction. | ||
| This journal is © The Royal Society of Chemistry 2024 |