Yong Yan *, Jie Li , Shasha Li , Mengna Wang , Gaoli Luo , Xiaohui Song , Suicai Zhang , Yurong Jiang , Ruiping Qin and Congxin Xia *
School of Physics, Henan Normal University, Xinxiang, Henan province, China. E-mail: yanyong@htu.edu.cn; xiacongxin@htu.edu.cn

Received 23rd August 2022 , Accepted 30th September 2022

First published on 3rd October 2022


Abstract

Germanium selenide (GeSe2), as a typical member of 2D wide bandgap semiconductors (WBSs), shows great potential in ultraviolet (UV) optoelectronics due to its excellent flexibility, superior environmental stability, competitive UV absorption coefficient, and significant spectral selectivity. However, the GeSe2-based UV photodetector suffers from high operation voltages and low photocurrent, which prevents its practical imaging applications. In this work, we report an elevated photocurrent generation in a vertical stacking graphene/GeSe2/graphene heterostructure with low operation voltage and low power consumption. Efficient collection of photoexcited carriers in GeSe2 through graphene electrodes results in outstanding UV detection properties, including a pronounced responsivity of 37.1 A W−1, a specific detectivity of 8.83 × 1011 Jones, and an ultrahigh on/off ratio (∼105) at 355 nm. In addition, building a Schottky barrier between GeSe2 and graphene and reducing the channel length can increase the photoresponse speed to ∼300 μs. These accomplishments set the stage for future optoelectronic applications of vertical 2D WBS heterostructure UV photodetectors.


Introduction

Advanced ultraviolet (UV) photodetectors that convert UV radiation signals into electronic signals are of great significance because they have extensive applications in the fields of military warning, spatial communication, ozone hole monitoring, and so on.1 In the past decades, wide-bandgap semiconductors (WBGSs), such as ZnO, TiO2, Ga2O3, and SnO2, have been used as excellent building blocks for UV optoelectronic devices with good responsivity, high specific detectivity, and low noise characteristics.2–6 However, the oxygen-related hole-trapping state induces a low response speed and poor anti-disturb ability, owing to the large density of defects and dangling bonds at the surface.7 Recently, 2D wide-bandgap semiconductors (2D WBGSs) have attracted significant attention because of their dangling-bond-free surfaces.8 For example, Ga2In4S9,9 NiPS3,10 GaPS4,11 and BiOBr12 are potential candidate materials for UV photodetectors. However, the synthesis is usually difficult and expensive owing to the complex chemical composition and structural polymorphism of these materials. It is known that elemental or binary compounds can be a more efficient choice for the preparation of detectors. For instance, hexagonal boron nitride (h-BN) with a direct wide bandgap of 5.9 eV, large absorption coefficient (7.5 × 105 cm−1), superior chemical inertness, shows a promising role in UV photodetection.12,13

2D WBGS germanium diselenide, GeSe2, attracts considerable attention due to its excellent anisotropic properties, high stability, strong nonlinearity, and fast response.14 Moreover, single layer GeSe2 has [GeSe4] tetrahedrons as the basic building blocks. The tetrahedrons form [GeSe4]n chains by corner-sharing along the a-axis, which are connected by [Ge2Se8] double tetrahedra by edge-sharing along the b-axis, forming an in-plane anisotropic geometry.15 Zhou et al. experimentally verified strong in-plane anisotropic properties of the rhombic GeSe2 layer.14 Additionally, Yang et al. demonstrated the weak interlayer interaction in GeSe2.16 It is well known that the electronic and optical properties of 2D materials are dependent on the layer number from multilayer to monolayer. Recently, exfoliated monolayer GeSe2 nanosheets have been found to have a direct bandgap of 2.96 eV.17 Meanwhile, GeSe2 is a well-defined p-type semiconductor with a hole mobility of 690 cm2 V−1 s−1, which is higher than that of most 2D semiconductors.18 However, the GeSe2 photodetector shows an ultralow photocurrent (∼pA) potentially retarding its practical application in UV detection, which is still required to be comprehensively improved.

In this study, we constructed a vertical GeSe2-based heterostructure with graphene (labeled as Gr) electrodes for high-performance UV photodetection. We systematically discussed the carrier transport mechanism in Gr/GeSe2/Gr devices, including direct tunneling (DT) to thermionic emission (TE) transport. The redistribution of space charge is increased by the external electric field, which improves the carrier collection efficiency. Moreover, the graphene electrode enhances the carrier extraction, resulting in an excellent photoresponse with a high responsivity of 7.6 × 103 mA W−1, a detectivity of 5.0 × 1010 Jones, a large on/off ratio (∼105), and a fast response speed of ≈0.3 ms under 405 nm laser irradiation. These results provide a scientific approach that directs a valuable way to prepare high-performance UV photodetectors.

Experimental details

Transfer method and device fabrication

Bulk GeSe2 crystals were synthesized by a chemical vapor transport method.17 The 2D GeSe2 flakes were achieved by mechanical exfoliation from bulk crystals with a polydimethylsiloxane (PDMS, Shanghai Onway Technology Co. Ltd) stamp-assisted peeling method.11 High-quality 90 nm SiO2/p+-Si wafer was used as the substrate. For better material adhesion, the substrate was placed on the micro heater of the transfer platform during the transfer process, and after aligning and placing the graphene in the center of the substrate and the temperature was ramped up to 80 °C, the PDMS stamp was allowed to adhere to the SiO2 surface. The temperature was then cooled down to 40 °C to release the glass slide and PDMS stamp from the SiO2/p+-Si substrate, leaving only the graphene flakes on top of the substrate. Following the same transfer procedure, the exfoliated GeSe2, and graphene were stacked layer by layer forming a Gr/GeSe2/Gr vertical vdW heterostructure. Finally, the devices were annealed at 150 °C for 3 h in a vacuum chamber. Standard photolithography was employed to define the source and drain electrode patterns on the wafer, and a 40 nm Au film was evaporated as the contact metal.

Characterization and measurements

The thickness of 2D nanosheets was identified by optical microscopy and atomic force microscopy (AFM, Dimension Icon, Bruker) in a tapping mode. The Raman spectrum was measured by confocal Raman microscopy (Horiba, Evolution HR, 532 nm laser excitation at room temperature). The elemental analysis was proceeded using SEM (SUPRA40, Carl Zeiss AG) combined with energy-dispersive spectrometry (EDS). The electronic and photoelectronic measurements were performed on a probe station (450PM, Micromanipulator) equipped with a semiconductor characterization system (B1500A, Keysight).

Results and discussion

Fig. 1a shows the schematic diagram of the Gr/GeSe2/Gr FET device, in which a GeSe2 layer is sandwiched between two cross-stacked metallic Gr layers on a 90 nm SiO2/p+-Si wafer. The 2D layers were mechanically exfoliated from GeSe2 and graphite crystals using the polydimethylsiloxane (PDMS) tape. The top and bottom graphene layers serve as the source and drain electrodes, respectively. The device was encapsulated with hexagonal boron nitride (hBN) layers, avoiding carrier scattering caused by adsorbents and impurities between the vertical heterostructure and insulating the device from the air.19 The overlapping area is 16.8 × 7.2 μm2 and the thickness (d) of the GeSe2 active layer is 70.3 nm. The Raman spectra in Fig. 1c were taken from points A, B, and C, respectively. Three Raman peaks at 95, 116, and 210 cm−1 correspond to the Ag typical vibrational modes of β-GeSe2.20,21 There is no detectable change in the GeSe2 peak position at different positions, indicating no mutual stress effect at the van der Waals interface. The G (1583 cm−1) and 2D (2748 cm−1) peaks were observed at the bottom Gr (9.8 nm, blue line) and the top Gr (4.3 nm, red line) layers, respectively.22 In addition, the detected stoichiometric ratio of Ge and Se is about 1[thin space (1/6-em)]:[thin space (1/6-em)]2 (Fig. S1). These results confirmed we prepared a high-quality Gr/GeSe2/Gr device by the dry transfer process.
image file: d2na00565d-f1.tif
Fig. 1 Schematic illustration (a) and optical micrograph (b) of the device with a multilayer GeSe2 semiconductor sandwiched between the T-Gr and B-Gr electrodes. (c) Raman spectra were collected from points A, B, C, bottom Gr, and top Gr, respectively.

We first investigated the current–voltage (IV) characteristics of the GeSe2 device with the drain bias voltage sweeping from 0 to ±5 V. The thickness of the GeSe2 layer was about 70.3 nm (Fig. S2). A Schottky contact was formed between semi-metallic Gr and 2D GeSe2 (Fig. 2a), which is similar to the contact between Gr and GaN.23 There are three ways for the charge to be transported through the Schottky barrier: DT, TE, and FN mechanisms.19,24–28 When −0.5 V < Vds <1.5 V, the current (at ∼pA) satisfies the DT mechanism. The carrier transport schematic is shown in Fig. 2e(i). Electrons cannot move across the barrier and only a few carriers can pass through the DT process, generating a small current. The direct tunneling process can be described by19,29

 
image file: d2na00565d-t1.tif(1)
 
image file: d2na00565d-t2.tif(2)
where d is the tunneling barrier thickness and fB is the tunneling barrier. Fig. 2a shows the linear ln(1/V) − ln(I/V2) curve, which is in agreement with the DT mechanism. When Vds > 1.5 V or Vds < −0.5 V, in Fig. 2a, the ln[thin space (1/6-em)]IV curve exhibits a linear shape (Fig. S2), indicating that charge carriers follow the TE mechanism. The TE mechanism shows the relationship between the current and voltage as shown by30
 
image file: d2na00565d-t3.tif(3)
 
image file: d2na00565d-t4.tif(4)
where A* is the effective Richardson's constant (A* = 4πm*qk02/h3, m* is the effective carrier mass), q is the unit electron charge, k0 is the Boltzmann constant, T is temperature, fB is the effective barrier height, and V is the bias voltage. n is the ideality factor. The slope is equal to e/nkT and allows one to extract the ideality factor n using
 
image file: d2na00565d-t5.tif(5)


image file: d2na00565d-f2.tif
Fig. 2 (a) IV characteristics of the thick GeSe2 (d = 70.3 nm) device, the black and red lines are in linear and logarithmic coordinates, respectively. (b) ln(I/V2) vs. ln(Vds−1) plot for the DT behavior. The top panel shows the tunneling current when the drain bias is between −0.5 and 0 V, and the bottom panel shows the tunneling current when the drain bias is between 0 and 1.5 V. (c) IV characteristics of the GeSe2 (d = 5.9 nm) device. (d) ln(I/V2) vs. 1/V plot (Fowler–Nordheim tunneling plot) when the drain bias is lower than −0.45 V. (e) Schematic illustration of the band diagrams.

Thus, the ideality factor n is 14.3. According to the Shockley–Read–Hall (SRH) recombination theory, the ideality factor of the recombination current is predicted to be n = 2 or less, which assumes recombination via isolated point defect levels. The larger ideality factor suggests other recombination currents crossing this Schottky junction.

As the physical properties of 2D materials are sensitive to thickness, we further explored the electrical performance of the device with thin GeSe2 (5.9 nm). When 0 V < Vds < 0.5 V, similar to the thick devices also have DT and TE processes (Fig. S2). For larger voltage biases (>0.5 V), FN tunneling is expected to dominate the charge transport. In the FN tunneling mechanism, the tunneling potential is modulated into a triangle barrier and the tunneling current can be described as19

 
image file: d2na00565d-t6.tif(6)
 
image file: d2na00565d-t7.tif(7)

In Fig. 2d, the ln(I/V2) − 1/V curve is linear with a slope image file: d2na00565d-t8.tif. The effective mass of the hole in the GeSe2 tunneling barrier can be extracted by its band structure fitting as m* = 1.8m0.20 The tunneling barrier height fB can be estimated to be 0.45 eV, confirming the FN tunneling behavior of the hole. The band alignment of Gr/GeSe2 heterostructures shows that the conduction and valence band offsets are 2.25 eV and 0.45 eV, respectively. (Fig. S3) With the large bias voltage, the energy band renders very strong bending, leading to a shift in transport mechanisms, in which holes can inject into the GeSe2 valence bands.

The optoelectronic properties of the device were then systematically studied to examine its potential application in UV photodetection. Fig. 3a and b present the IV characterization of the devices based on the GeSe2 thickness-modulation (the corresponding optical images are shown in Fig. S4). The different current densities are ascribed to the GeSe2 thickness and tunnel junction area. We calculated the current density (J) to normalize the influence of the tunnel area. For the case of the thinnest sample (9.8 nm), the device exhibited a high dark current. As we discussed above, DT is the dominant carrier transport mechanism under small Vds. The tunneling probability (PTB) is evaluated based on the equation31

 
image file: d2na00565d-t9.tif(8)
where ℏ is the reduced Planck's constant, m is the mass of the free carrier, and wTB and ΦTB are the width and height of the potential barrier. There is a bandgap difference of only 0.26 eV between the monolayer and bulk GeSe2.17 The tunneling probability can be suspected in terms of the barrier width, that is, the thickness. Therefore, the thinner GeSe2 vertical device shows a larger dark current.


image file: d2na00565d-f3.tif
Fig. 3 The optoelectronic performances of the GeSe2 devices with different thicknesses. (a) JV logarithm plots for the dark state (dashed line) and 405 laser irradiation (solid line). (b) PDCR, responsivity (R), External Quantum Efficiency (EQE), detectivity (D), gain (G) extracted from (a).

Under 405 nm light illumination, all devices exhibit a positive photoresponse because the photon absorption generates electron–hole pairs in GeSe2 layers, which drift in opposite directions towards the graphene electrode. To evaluate the performance of photodetectors, several important parameters are explored quantitatively, including photo-to-dark-current ratio (PDCR), response (Rλ), external quantum efficiency (EQE), and detectivity (D*). They are defined as32–34

 
image file: d2na00565d-t10.tif(9)
 
Rλ = Iph/PinS(10)
 
EQE = hcRλ/(11)
 
image file: d2na00565d-t11.tif(12)
 
image file: d2na00565d-t12.tif(13)
where Iph is the photocurrent (IilluminationIdark), Pin is the light power intensity, S is the area of the overlapped region, h is the Planck constant, c is the velocity of light, λ is the wavelength of exciting light, L is the length of the channel (GeSe2 thickness), and μ is the carrier mobility. The 26.8 nm GeSe2 device exhibits a better photoresponse with PDCR = 83.3, Rλ = 7.6A/W, EQE = ∼2316%, and D* = 5.0 × 1010 Jones. In general, a thicker sample has a higher absorption coefficient than a thinner one, producing a larger photocurrent. However, it has been reported that an increase in absorption layer thickness will result in a decrease in current gain. The reason is that increasing the thickness uniformly reduces the electric field intensity, resulting in significant reduction in the field-effect drifting of electrons and holes. Consequently, it is still essential to optimize the thickness of GeSe2 layers to function as light absorption and charge separation layers in the future.

To validate the superiority of this Gr/GeSe2/Gr vertical device, one set of comparisons between vertical and planar devices is shown in Fig. 4. The optoelectrical performance of vertical devices is much better than that of the planar device. The short transport channel results in a large electric field, leading to a highly efficient separation for the majority carriers and a high photocurrent. In addition, the vertical device with graphene electrodes shows better performance than that of the device with Au electrodes, which is ascribed to the UV light absorbance of Au electrodes reducing the carrier generation in the GeSe2 layer. Therefore, in Gr/GeSe2/Gr devices, the stronger input light and high carrier mobility of Gr layers lead to the devices showing excellent optoelectronic performance which is two orders of magnitude higher than those of the other architectures (see ESI Material Fig. S5 for details).


image file: d2na00565d-f4.tif
Fig. 4 The electrical performance of three photodetectors with different architectures: (a) Gr/GeSe2/Gr (vertical), (b) Au/GeSe2/Au (vertical), and (c)Au/GeSe2/Au (horizontal), respectively. The inset diagram shows the structure schematic and band diagram.

To demonstrate the spectrum-selective UV photodetection capability of our device, a series of photoelectric measurements were performed at different wavelengths. The time-resolved photoresponse at various wavelengths under the same light power (10 nW) is shown in Fig. 5a. These spectral photocurrent curves indicate an obvious suppression of device responsivity beyond the UV range. Fig. 5b shows the gradual increase in photocurrent with increasing illumination power density. Under an incident light of 2.7 mW cm−2, the Ilight/Idark ratio has already reached over 1.12 × 105. The photocurrent can be expressed by a power law relationship IphP0.91, as shown in Fig. 5c, suggesting efficient electron–hole pair generation and separation in the GeSe2 layers and Gr/GeSe2 Schottky interface.


image file: d2na00565d-f5.tif
Fig. 5 (a) Photocurrent–time (It) response at various wavelengths. (b) It response (fixed dc bias: 1 V) under a 405 nm laser with different power intensities. (c) Photocurrent as a function of light power density at Vds = 1 V. (d) A typical photoresponse time curve for the rise time and the fall time. (e) Stability testing. (f) Anisotropic photoresponse under a 405 nm laser.

The response speed is another pivotal parameter for PDs. We use the rise time (τr) and decay time (τd) to describe the response speed. The τr and τd are defined as the times of current changing between 10% and 90% of the maximum value, respectively. Importantly, the τr and τd are about 300 μs and 350 μs, which are measured using a home-made system with a voltage of 0.916 V. The system consists of a laser, an optical microscope, a current amplifier, and an oscilloscope. These values are smaller than those of lateral GeSe2 and Ga2O3 PDs. The ultrafast photoresponse of this photodetector is mainly attributed to a strong electric field at the junction between the Gr electrodes and GeSe2 layers, where carriers are spontaneously transferred. The anisotropy of the crystal structure and geometry of GeSe2 nanoflakes will directly lead to the anisotropy of photoelectric transport of carriers. Linearly polarized photodetection was investigated in Fig. 5f under 405 nm polarization illumination. It is clear that by rotating the polarization of the light, the photocurrent changes dramatically. These results further confirm that the photocurrent comes from the GeSe2 layer, which offers us a great opportunity to further exploit GeSe2 in the practical polarization-sensitive photodetector. Table 1 summarizes the performance of the Gr/GeSe2/Gr heterojunction photodetector and some reported photodetectors based on wide bandgap 2D nanomaterials for comparison. Notably, the performances of the Gr/GeSe2/Gr heterojunction photodetector in our work are better than those of the reported wide bandgap 2D nanomaterial-based photodetectors.

Table 1 Summary of 2D wide bandgap photodetectors
Materials Measurement condition R [mA W−1] EQE [%] D* [Jones] Response time [ms] On/off ratio Ref
GeSe2 355 nm @ 1 V 3.7 × 104 11[thin space (1/6-em)]300 8.83 × 1011 0.3/0.35 >105 This work
405 nm @ 1 V 7.6 × 103 2316 5.0 × 1010
CdS 400 nm @ 2 V 0.18 × 103 55.87 2.7 × 109 14/8 103 35
GaN 325 nm @ 2 V 1367 152.4/155.3 29.09 36
CaS 254 nm @ 2 V 4.2 × 103 2050 1013 37
4H–SiC 310 nm @ 5 V 70 33 38
Ga2In4S9 360 nm @ 5 V 111.9 × 103 3.85 × 104 2.25 × 1011 40/50 2136 9
WS2 365 nm @ 5 V 53.3 × 103 1.22 × 1011 30 2.94 × 104 39
AlN 180 nm @ 5 V 110/80 102 32
GQD 254 nm @ 5 V 2.1 9.59 × 1011 64/43 6000 40
ZnS 320 nm @ 5 V 120 50 41
CaTe 375 nm @ 5 V 30 54 42
SnS2 405 nm @ 5 V 0.695 0.22 7.39 × 106 400 43
Diamond 210 nm @ 5 V 48 42 44
NiPS3 254 nm @10 V 126 1.22 × 1012 453/384 2 × 102 10
BiOBr 315 nm @ 10 V 12739 × 103 6.46 × 106 8.37 × 1012 0.102 104 12
CuGaS2 254 nm @ 10 V 5.1 × 103 1.67 × 1011 1800/10[thin space (1/6-em)]100 45
Ga2O3 250 nm @ 10 V 37 18 103 6
TiO2 310 nm @ 10 V 3.27 4
ZnMgO 260 nm @ 10 V 1.664 46
GeSe2 266 nm @ 20 V 200 93 1.6 × 1015 300 100 17
h-BN 212 nm @ 20 V 0.1 2.4 × 108 320/630 103 13
CuBr 345 nm @ 30 V 3.17 × 103 1126 1.4 × 1011 32/48 47


Conclusion

In summary, we have fabricated a series of planar and vertical devices based on GeSe2 and Gr layers. Optical microscopy, AFM, Raman spectroscopy, and photoelectric measurements were systematically performed. The carrier transport mechanism of direct tunneling and thermoelectric emission was analyzed in the Gr/GeSe2/Gr device. Compared with the vertical Au/GeSe2/Au, horizontal Au/GeSe2/Au, and other 2D material photodetectors, the vertical Gr/GeSe2/Gr exhibits competitive high performance including an excellent responsivity of 37.1 A W−1, a maximum detectivity of 8.83 × 1011 Jones, a high on/off ratio (∼105) at 355 nm, and a fast response time of ∼300 μs. We believe that the GeSe2-based vertical heterostructure will be a good candidate for application in UV photoelectronics.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

This work was supported by the Natural Science Foundation of China under Grant No. 61804047, the Training Program for the National Foundation of Henan Normal University (Grant No. 2017PL02), the HPCC of Henan Normal University, the National Natural Science Foundation of China (Grant No. 12074103), the Program for Science & Technology Innovation Talents in University of Henan Province (Grant No. 202300410221), the Henan Province Universities Scientific Research Key Project (No. 21A140015), and the Henan Innovative science and technology team (CXTD2017080). Also, this work was supported by “The Pearl River Talent Recruitment Program” (2019ZT08X639).

References

  1. H. Chen, K. Liu, L. Hu, A. A. Al-Ghamdi and X. Fang, Mater. Today, 2015, 18, 493–502 CrossRef CAS .
  2. S. Mitra, Y. Pak, N. Alaal, M. N. Hedhili, D. R. Almalawi, N. Alwadai, K. Loganathan, Y. Kumarasan, N. Lim, G. Y. Jung and I. S. Roqan, Adv. Opt. Mater., 2019, 7, 1900801 CrossRef CAS .
  3. C. Tong, J. Yun, E. Kozarsky and W. A. Anderson, J. Electron. Mater., 2013, 42, 889–893 CrossRef CAS .
  4. H. Huang, Y. Xie, Z. Zhang, F. Zhang, Q. Xu and Z. Wu, Appl. Surf. Sci., 2014, 293, 248–254 CrossRef CAS .
  5. A. Das Mahapatra and D. Basak, Sens. Actuators, A, 2020, 312, 112168 CrossRef CAS .
  6. T. Oshima, T. Okuno and S. Fujita, Jpn. J. Appl. Phys., 2007, 46, 7217–7220 CrossRef CAS .
  7. B. Nabet, Photodetectors: Materials, Devices and Applications in Communications and Imaging Technologies, Elsevier Science & Technology, 2015 Search PubMed .
  8. O. Lopez-Sanchez, D. Lembke, M. Kayci, A. Radenovic and A. Kis, Nat. Nanotechnol., 2013, 8, 497–501 CrossRef CAS PubMed .
  9. F. Wang, T. Gao, Q. Zhang, Z. Y. Hu, B. Jin, L. Li, X. Zhou, H. Li, G. Van Tendeloo and T. Zhai, Adv. Mater., 2019, 31, 1806306 CrossRef PubMed .
  10. J. Chu, F. Wang, L. Yin, L. Lei, C. Yan, F. Wang, Y. Wen, Z. Wang, C. Jiang, L. Feng, J. Xiong, Y. Li and J. He, Adv. Funct. Mater., 2017, 27, 1701342 CrossRef .
  11. Y. Yan, J. Yang, J. Du, X. Zhang, Y. Y. Liu, C. Xia and Z. Wei, Adv. Mater., 2021, 33, 2008761 CrossRef CAS PubMed .
  12. C. Gong, J. Chu, S. Qian, C. Yin, X. Hu, H. Wang, Y. Wang, X. Ding, S. Jiang, A. Li, Y. Gong, X. Wang, C. Li, T. Zhai and J. Xiong, Adv. Mater., 2020, 32, 1908242 CrossRef CAS PubMed .
  13. H. Liu, J. Meng, X. Zhang, Y. Chen, Z. Yin, D. Wang, Y. Wang, J. You, M. Gao and P. Jin, Nanoscale, 2018, 10, 5559–5565 RSC .
  14. X. Zhou, X. Hu, S. Zhou, Q. Zhang, H. Li and T. Zhai, Adv. Funct. Mater., 2017, 27, 1703858 CrossRef .
  15. X. W. Zongbao Li, W. Shi, X. Xing, D.-J. Xue and J.-S. Hu, RSC Adv., 2018, 8, 33445 RSC .
  16. Y. Yang, X. Wang, S. C. Liu, Z. Li, Z. Sun, C. Hu, D. J. Xue, G. Zhang and J. S. Hu, Adv. Sci., 2019, 6, 1801810 CrossRef PubMed .
  17. Y. Yan, W. Xiong, S. Li, K. Zhao, X. Wang, J. Su, X. Song, X. Li, S. Zhang, H. Yang, X. Liu, L. Jiang, T. Zhai, C. Xia, J. Li and Z. Wei, Adv. Opt. Mater., 2019, 7, 1900622 CrossRef CAS .
  18. M. Cao, B. Cheng, Li. Xiao, J. Zhao, X. Su, Y. Xiao and a. S. Leia, J. Mater. Chem. C, 2015, 3, 5207 RSC .
  19. L. Tong, M. Peng, P. Wu, X. Huang, Z. Li, Z. Peng, R. Lin, Q. Sun, Y. Shen, X. Zhu, P. Wang, J. Xu and L. Ye, Sci. Bull., 2021, 66, 139–146 CrossRef CAS .
  20. Y. Yang, S. C. Liu, W. Yang, Z. Li, Y. Wang, X. Wang, S. Zhang, Y. Zhang, M. Long, G. Zhang, D. J. Xue, J. S. Hu and L. J. Wan, J. Am. Chem. Soc., 2018, 140, 4150–4156 CrossRef CAS PubMed .
  21. H. Ouyang, S.-Y. Hu, M.-L. Shen, C.-X. Zhang, X.-A. Cheng and T. Jiang, Acta Phys. Sin., 2020, 69, 184212 CrossRef .
  22. A. C. Ferrari, J. C. Meyer, V. Scardaci, C. Casiraghi, M. Lazzeri, F. Mauri, S. Piscanec, D. Jiang, K. S. Novoselov, S. Roth and A. K. Geim, Phys. Rev. Lett., 2006, 97, 187401 CrossRef CAS PubMed .
  23. Z. A. Ansari, T. J. Singh, S. M. Islam, S. Singh, A. K. Pramila Mahala and K. J. Singh, Optik, 2019, 182, 500 CrossRef CAS .
  24. J. M. Beebe, B. Kim, J. W. Gadzuk, C. D. Frisbie and J. G. Kushmerick, Phys. Rev. Lett., 2006, 97, 026801 CrossRef PubMed .
  25. S.-J. Liang and L. K. Ang, Phys. Rev. Appl., 2015, 3, 014002 CrossRef CAS .
  26. S. Pandey, C. Biswas, T. Ghosh, J. J. Bae, P. Rai, G. H. Kim, K. J. Thomas, Y. H. Lee, P. Nikolaev and S. Arepalli, Nanoscale, 2014, 6, 3410–3417 RSC .
  27. T. Ikuno, H. Okamoto, Y. Sugiyama, H. Nakano, F. Yamada and I. Kamiya, Appl. Phys. Lett., 2011, 99, 023107 CrossRef .
  28. C. Kim, I. Moon, D. Lee, M. S. Choi, F. Ahmed, S. Nam, Y. Cho, H. J. Shin, S. Park and W. J. Yoo, ACS Nano, 2017, 11, 1588–1596 CrossRef CAS PubMed .
  29. X. Zhou, X. Hu, S. Zhou, H. Song, Q. Zhang, L. Pi, L. Li, H. Li, J. Lu and T. Zhai, Adv. Mater., 2018, 30, 1703286 CrossRef PubMed .
  30. Y. Sun, Z. Jiao, H. J. W. Zandvliet and P. Bampoulis, J. Phys. Chem. C, 2022, 126, 11400–11406 CrossRef CAS PubMed .
  31. H. Su, T. Hu, F. Wu and E. Kan, J. Phys. Chem. C, 2021, 125, 10738–10746 CrossRef CAS .
  32. D. S. Tsai, W. C. Lien, D. H. Lien, K. M. Chen, M. L. Tsai, D. G. Senesky, Y. C. Yu, A. P. Pisano and J. H. He, Sci. Rep., 2013, 3, 2628 CrossRef PubMed .
  33. F. Yan, Z. Wei, X. Wei, Q. Lv, W. Zhu and a. K. Wang, Small Methods, 2018, 2, 1700349 CrossRef .
  34. M. Buscema, J. O. Island, D. J. Groenendijk, S. I. Blanter, G. A. Steele, H. S. van der Zant and A. Castellanos-Gomez, Chem. Soc. Rev., 2015, 44, 3691–3718 RSC .
  35. B. Jin, P. Huang, Q. Zhang, X. Zhou, X. Zhang, L. Li, J. Su, H. Li and T. Zhai, Adv. Funct. Mater., 2018, 28, 1800181 CrossRef .
  36. R. Yu, G. Wang, Y. Shao, Y. Wu, S. Wang, G. Lian, B. Zhang, H. Hu, L. Z. Lei Liu and a. X. Hao, J. Mater. Chem. C, 2019, 7, 14116–14122 RSC .
  37. P. Hu, L. Wang, M. Yoon, J. Zhang, W. Feng, X. Wang, Z. Wen, J. C. Idrobo, Y. Miyamoto, D. B. Geohegan and K. Xiao, Nano Lett., 2013, 13, 1649–1654 CrossRef CAS PubMed .
  38. Y.-Z. Chiou, Jpn. J. Appl. Phys., 2004, 43, 2432–2434 CrossRef CAS .
  39. L. Zeng, L. Tao, C. Tang, B. Zhou, H. Long, Y. Chai, S. P. Lau and Y. H. Tsang, Sci. Rep., 2016, 6, 20343 CrossRef CAS PubMed .
  40. Q. Zhang, J. Jie, S. Diao, Z. Shao, Q. Zhang, L. Wang, W. Deng, W. Hu, H. Xia, X. Yuan and a. S.-T. Lee, IEEE, 2015, 9, 1561–1570 CAS .
  41. X. Fang, Y. Bando, M. Liao, U. K. Gautam, C. Zhi, B. Dierre, B. Liu, T. Zhai, T. Sekiguchi, Y. Koide and D. Golberg, Adv. Mater., 2009, 21, 2034–2039 CrossRef CAS .
  42. Z. Wang, M. Safdar, M. Mirza, K. Xu, Q. Wang, Y. Huang, F. Wang, X. Zhan and J. He, Nanoscale, 2015, 7, 7252–7258 RSC .
  43. Jia-Jing Wu, Y.-R. Tao, Yi. Wu and X.-C. Wu, Sens. Actuators, A, 2016, 231, 211–217 CrossRef CAS .
  44. A. BenMoussa, A. Soltani, K. Haenen, U. Kroth, V. Mortet, H. A. Barkad, D. Bolsee, C. Hermans, M. Richter, J. C. De Jaeger and J. F. Hochedez, Semicond. Sci. Technol., 2008, 23, 035026 CrossRef .
  45. B. Xin, Y. Wu, X. Liu, N. Zhang, H. Yu and W. Feng, Semicond. Sci. Technol., 2019, 34, 055007 CrossRef CAS .
  46. M. M. Fan, K. W. Liu, Z. Z. Zhang, B. H. Li, X. Chen, D. X. Zhao, C. X. Shan and D. Z. Shen, Appl. Phys. Lett., 2014, 105, 011117 CrossRef .
  47. C. Gong, J. Chu, C. Yin, C. Yan, X. Hu, S. Qian, Y. Hu, K. Hu, J. Huang, H. Wang, Y. Wang, P. Wangyang, T. Lei, L. Dai, C. Wu, B. Chen, C. Li, M. Liao, T. Zhai and J. Xiong, Adv. Mater., 2019, 31, 1903580 CrossRef PubMed .

Footnote

Electronic supplementary information (ESI) available. See https://doi.org/10.1039/d2na00565d

This journal is © The Royal Society of Chemistry 2022