Temperature-dependent modulation by biaryl-based monomers of the chain length and morphology of biphenyl-based supramolecular polymers

Tomokazu Iseki ab, Mathijs F. J. Mabesoone ac, Mark A. J. Koenis d, Brigitte A. G. Lamers a, Elisabeth Weyandt a, Lafayette N. J. de Windt a, Wybren Jan Buma de, Anja R. A. Palmans a and E. W. Meijer *a
aInstitute for Complex Molecular Systems and Laboratory of Macromolecular and Organic Chemistry, Eindhoven University of Technology, 5600 MB Eindhoven, The Netherlands. E-mail: e.w.meijer@tue.nl
bMaterial Science Research Laboratory, Kao Corporation, Wakayama-shi, Wakayama 640-8580, Japan
cInstitute of Microbiology, Eidgenössische Technische Hochschule Zürich, Vladimir-Prelog-Weg 4, 8093 Zurich, Switzerland
dVan't Hoff Institute for Molecular Sciences, University of Amsterdam, Science Park 904, 1098 XH Amsterdam, The Netherlands
eInstitute for Molecules and Materials, FELIX Laboratory, Radboud University, Toernooiveld 7c, 6525 ED Nijmegen, The Netherlands

Received 20th July 2021 , Accepted 6th September 2021

First published on 6th September 2021


Abstract

Supramolecular copolymerizations offer attractive options to introduce structural and functional diversity in supramolecular polymer materials. Yet, general principles and structure–property relationships for rational comonomer design remain lacking. Here, we report on the supramolecular (co)aggregation of a phenylpyridine and bipyridine derivative of a recently reported biphenyl tetracarboxamide-based monomer. We show that both arylpyridines are poor monomers for supramolecular homopolymerizations. However, the two arylpyridines efficiently influence supramolecular polymers of a biphenyl-based polymer. The phenylpyridine derivatives primarily sequestrate biphenyl monomers, while the bipyridine intercalates into the polymers at high temperatures. Thereby, these two poorly homopolymerizing monomers allow for a fine control over the length of the biphenyl-based supramolecular polymers. As such, our results highlight the potential to control the structure and morphology of supramolecular polymers by tailoring the electronic properties of additives.


Introduction

Additives play a central role in tailoring material properties in both synthetic and natural systems. In synthetic polymeric materials chain transfer agents1–3 or plasticizers4–6 alter the material at a microscopic and macroscopic level, respectively. A related role is played by additives that in some cases do not polymerize themselves but are great comonomers like in polystyrene-maleimide. In addition, copolymers, such as glycosaminoglycans,7–9 and repeating peptide sequences, as observed in e.g. silks,10–12 are important for many biomaterials.

Supramolecular polymers occupy a central role in this regard, as the dynamic nature of these materials holds great promise for integration into biological systems, while also providing attractive properties for optoelectronic applications and recycling of plastics. Seminal contributions are presented by Aida13–15 and Stupp16–18 for electronic and biological applications, respectively, while our group focused on mechanical properties.19 However, despite a few decades of research, the development of design principles to control the structure of supramolecular materials with small amounts of comonomers and/or additives is still in its infancy.20–23

From all the supramolecular polymers introduced so far, the cooperative polymerization of hydrogen-bonded disk-like molecules into helical one-dimensional aggregates, has been studied in most detail. The focus in supramolecular copolymerizations in this class was initially limited to fundamental stereochemical studies in so-called sergeant-and-soldiers24–26 and majority-rules27–30 experiments. Recent years have shown a strong interest in diversifying polymeric structure and the introduction of function through copolymerizations. Supramolecular block copolymers,31–34 as well as alternating35 and random copolymers36 have been reported for a wide range of discotic monomers. Complementing the experimental work with theoretical and computational methods, such as mass-balance37 and statistical mechanical models35 or molecular dynamics simulations,38,39 has shown to be crucial for a full interpretation of the results. In most of the systems reported, the employed comonomers are of comparable chemical nature, which facilitates incorporation of one monomer into aggregates of the other. Porphyrins form a notable exception to this observation, since complexation of small ligands to metallated porphyrins only occurs on free monomers or on chain ends of the supramolecular polymer.40–44 As a result, only a handful of chain cappers or sequestrators have been successfully designed45–50 and the current lack of general principles to rationally designed comonomers in supramolecular polymers impedes further application of these functionally diverse materials.

In our search for fundamental principles that determine the role of comonomers and additives in supramolecular polymerizations, we were inspired by the potential for electronically diverse monomer scaffolds offered by the biaryl tetracarboxamide platform we reported recently.51 This biphenyl-tetracarboxamide-based monomer ((S)-BPTA, Fig. 1) forms supramolecular polymers in apolar solvents such as methylcyclohexane (MCH). Upon binding minute amounts of codissolved monomeric water,52(S)-BPTA-based supramolecular polymers show remarkable structural transformations. Moreover, we showed that small steric variations in the aliphatic side chain of (S)-BPTA can lead to various unforeseen, ‘abnormal’ sergeants-and-soldiers effects, highlighting the delicate energy balances that operate in supramolecular copolymerizations.53 We envision that further control over and diversity in the supramolecular architecture of BPTA-based polymers can be obtained, not by tuning peripheral steric interactions, but rather by controlling electronic interactions at the core of the polymer.23 To this end, we designed two new biaryl analogues, i.e. the tetracarboxamides of 4-phenylpyridine and 4,4′-bipyridine (PhePyTA and BiPyTA, respectively, see Fig. 1).


image file: d1sc03974a-f1.tif
Fig. 1 Chemical structures of the (S)-BPTA, (S) and (R)-PhePyTA and (S)-BiPyTA compounds used in this study.

Here, we first disclose the scope and limitations of the homopolymerization of both PhePyTA and BiPyTA. We show that PhePyTA can assemble into two different types of supramolecular polymers at high concentrations, one of which is dependent on the presence of water. The less-soluble BiPyTA assembles into a single type of supramolecular polymer already at low concentration. Next, we investigate the effect of these electron-deficient analogues in the copolymerization of (S)-BPTA with (S)-PhePyTA and (S)-BiPyTA. We find that both PhePyTA and BiPyTA can act as temperature-dependent chain-length modulators of the BPTA-based supramolecular copolymers. As such, tailoring electronic properties of additives may pave the way towards supramolecular polymer architectures as diverse as seen in covalent polymer science.

Results and discussion

Complete synthetic procedures and the full molecular characterization of the new monomers are given in the ESI.

Water modulates the length of PhePyTA-based aggregates

Bulk samples of monomer (S)-PhePyTA show no birefringence in polarized optical microscopy (POM) images and no phase transitions in differential scanning calorimetry (DSC). Only minor shifts in the variable temperature infrared (IR) spectrum and the absence of ordered structures, as indicated by small angle X-ray scattering (SAXS) (Fig. S1–S4), are observed. In contrast to the lack of supramolecular ordered structures in the bulk phase, solution-state SAXS experiments in ambient MCH solutions of (S)-PhePyTA show the formation of short cylindrical supramolecular polymers with a length of 54 nm and a radius of 6.6 nm. Upon increasing the concentration from 2 to 8 mM, the length of the polymers increases only slightly from 54 to 87 nm, indicating that the elongation constant of the polymerization might decrease with polymer length (Fig. S5).54 The absence of long, one-dimensional polymers is further corroborated by AFM experiments (Fig. S6). The weak increase in polymer length upon quadrupling the concentration suggests additional interactions that may truncate the supramolecular polymer. IR spectra show that, despite the absence of long, fibrillar structures, the structures formed by (S)-PhePyTA are stabilized by hydrogen bonding. Upon changing the solvent from CDCl3 to d14-MCH, a new band in the carbonyl stretch region emerges at 1641 cm−1 and the amide stretch vibrations move from 3491 to 3312 cm−1, respectively. The latter strongly indicates the formation of intermolecular hydrogen bonds (Fig. 2a). Interestingly, these IR bands show a dependency on the humidity of the MCH solvent, as was also observed in the strongly water-dependent polymerization of (S)-BPTA. However, the characteristic peak at 3558 cm−1, which is indicative of the incorporation of strongly hydrogen-bonded water in the supramolecular structure is absent. The broad feature between 3200 and 3600 cm−1 does suggest, however, that some hydrogen-bonded water may be present in the solution and around the substrate, but the water is not tightly bound to the supramolecular aggregates.
image file: d1sc03974a-f2.tif
Fig. 2 (a) FT-IR spectra of 2 mM solutions of (S)-PhePyTA in various solvents. (b) Experimental vibrational absorption (VA) (lower panel) and vibrational circular dichroism (VCD) (upper panel) spectra of 10 mM solutions of (R)- and (S)-PhePyTA in ambient MCH. (c) Comparison of experimental VA (lower panel) and VCD (upper panel) spectra of (S)-PhePyTA in ambient MCH with spectra calculated for ‘zig-zag’ aggregates. (d and e) Cartoons of the dominant ‘zig-zag’ (d) and minor helical (e) hydrogen bond pattern in (S)-PhePyTA aggregates.

Further insights into the structure of the aggregates formed by (S)-PhePyTA and its enantiomer under ambient conditions at room temperature, are obtained with VCD spectroscopy in combination with DFT calculations (Fig. 2b). Under these conditions, the system is above the water-dependent transition temperature (Fig. S7). The VCD spectra show strong features arising from coupled oscillators, thereby indicating that (S)-PhePyTA aggregates in an oligomeric or polymeric form of at least 2–4 molecules. A reasonable mirror symmetry between the spectra of (S)- and (R)-PhePyTA is obtained. The smaller signal intensity of (R)-PhePyTA can be explained by subtly different degrees of aggregation and/or enantiomeric excess. In contrast to other VCD experiments on supramolecular polymers,55–58 in which the bisignate VCD bands pointed to helical polymers, DFT calculations of VCD spectra of helically hydrogen-bonded (S)-PhePyTA did not give a good agreement with the spectra experimentally observed (Fig. 2c, e and S8). Remarkably, VCD spectra calculated for optimized geometries in which the amides are oriented in a ‘zig-zag’ fashion with stacks in a slight helical twist (Fig. 2d) showed considerably better overlap with the observed spectra (Fig. 2c). Our calculations under vacuum conditions show that this ‘zig-zag’ pattern is considerably lower in energy (17.6 kJ mol−1 for the trimer structures) than the helical hydrogen bonding pattern (Fig. 2d). Combined with the experimental results, the calculations indicate that in the water-free (S)-PhePyTA aggregates, the classical, helical organization of the hydrogen bonds is only a minor population. Rather, most hydrogen bonds in these aggregates are organized in the ‘zig-zag’ orientation.

This dominant ‘zig-zag’ conformation is corroborated by NOESY NMR experiments of (S)-PhePyTA at 80 °C in d14-MCH (Fig. S9). Here, the absence of a NOE peak between the pyridyl protons and the amides on the pyridine ring suggests the presence of an intramolecular hydrogen bond between the amides and the pyridine nitrogen.

We further investigated the supramolecular architectures formed by (S)-PhePyTA in MCH and their dependency on the water content by variable temperature circular dichroism (VT-CD) and UV-Vis (VT-UV) spectroscopy. At 85 °C in dry MCH, 510 μM solutions of (S)-PhePyTA show a broad, CD-silent absorption band below 350 nm with a maximum below 230 nm (Fig. 3a). This spectrum is similar to the spectrum observed for (S)-BPTA, but slightly redshifted. Upon cooling the solution below 60 °C, a weak CD spectrum showing a minimum around 275 nm emerges, while the absorption spectrum narrows slightly, indicating the formation of weakly ordered helical structures, which we label APhePyTA. Further cooling to 5 °C does not lead to further changes in the CD or UV spectra, indicating that the aggregates do not undergo further structural changes. In contrast, when ambient MCH solutions, containing 21–32 ppm H2O, are cooled below 20 °C, the CD spectrum strongly increases in intensity, while retaining its shape (Fig. 3b). Concurrently, the absorption spectrum shows further sharpening, indicating a transition from the APhePyTA state to a second aggregate state, which we label as BPhePyTA.


image file: d1sc03974a-f3.tif
Fig. 3 VT-CD and UV spectra recorded upon cooling 300 μM solutions of (S)-PhePyTA in dry (a) and ambient (b) MCH. Spectra are recorded at 5 °C intervals, with the red spectra being recorded at 85 °C and the blue spectra at −10 °C. The grayscale indicates the temperature gradient from high (light) to low (dark) temperature. (c) VT-CD traces at 266 nm for solutions containing various amounts of (S)-PhePyTA in MCH containing 21–31 ppm H2O (top panel) and 510 μM solutions containing various amounts of water (bottom panel). The sample containing 510 μM (S)-PhePyTA in the top panel contained 30 ppm water.

Similar to the water-dependent supramolecular polymerization of (S)-BPTA, the elongation temperature of monomeric (S)-PhePyTA into APhePyTA gradually decreases as the concentration is decreased but does not show a dependency on water content (Fig. 3c, top panel). In contrast, the transition between APhePyTA and BPhePyTA is independent of concentration, yet strongly affected by the water content (Fig. 3c, bottom panel). The temperature-dependent CD intensity of (R)-PhePyTA gives a mirror-image cooling curve with identical transition temperatures (Fig. S10). A van't Hoff analysis of the concentration-dependent elongation temperatures of (S)-PhePyTA extracted from the VT-UV traces reveals that the enthalpy and entropy changes upon formation of APhePyTA are −94 kJ mol−1 and −220 J mol−1 K−1, respectively (Fig. S11). The enthalpy released by (S)-PhePyTA upon aggregation is slightly more negative than the enthalpy released by (S)-BPTA,51 indicating that the dipolar character of the phenylpyridine core may stabilize the water-free APhePyTA state with respect to the A state of (S)-BPTA. During the transition from APhePyTA to BPhePyTA, all VT-CD intensities of the samples measured increase as the solutions are cooled to temperatures as low at −10 °C, indicating that the system does not fully transform from APhePyTA to BPhePyTA in the temperature range probed. Unfortunately, the incomplete transition to BPhePyTA does not allow us to extract the molar ellipticity of BPhePyTA, which prevents meaningful fitting to a solvent-dependent mass-balance model as was done for (S)-BPTA.51,53 Thus, the VT-CD and UV results show that the monomers in the competing APhePyTA and BPhePyTA states have similar molecular arrangements, but further insights into the water-dependent competition between APhePyTA and BPhePyTA are necessary for a complete description of the aggregation.

More details of the differences between APhePyTA and BPhePyTA were obtained with static light scattering techniques. For this, we probed the angle and temperature-dependent-scattering of an MCH solution saturated with water and containing 2 mM (S)-PhePyTA. The scattering profile below 20 °C, where BPhePyTA is stable, does not show any significant dependency on the angle-dependent scattering vector, indicating the presence of spherical or very short aggregates (Fig. 4a and S12). Upon heating from 20 to 40 °C, the count rate increases twofold and reaches a plateau between 40 and 60 °C. At this plateau, the angle independency is preserved over the entire q-range measured and is in line with the plateau observed at q-values below 0.05 nm−1 in the solution state SAXS measurements on APhePyTA (Fig. 4b and S12). Upon heating above 60 °C, the sample shows concomitant decreases in scattering intensity and CD intensity and above 80 °C, the sample hardly scatters and shows no CD signal (Fig. 4b).


image file: d1sc03974a-f4.tif
Fig. 4 (a) Dependency of the SLS count rate at 20 °C on the scattering vector, q, of a 2 mM (S)-PhePyTA solution MCH that is saturated with water. (b) VT-CD intensity at 266 nm (top panel) and count rates at a 90° scattering angle as observed by SLS (bottom panel) of a 2 mM (S)-PhePyTA solution in MCH saturated with water.

The concomitant changes in scattering and CD intensity provide valuable clues on the structures of the various (S)-PhePyTA aggregates. The initial increase in scattering intensity and decrease in CD signal upon heating the sample from 20 to 40 °C, together with the plateau observed in SAXS, indicates that the spherical or very short fibrillar structures present at room temperature, BPhePyTA, elongate into larger, but more disorganized fibrillar aggregates, APhePyTA. Interestingly water stabilizes the short fibrillar structures present at low temperature (Fig. 3c). Upon heating the samples, the water is released from the solvated BPhePyTA state. As BPhePyTA transitions to APhePyTA, an increase in the polymer length occurs, as has been observed before in several systems containing hydrogen-bond competitors, such as water and alcohols.59–64 In contrast to the previously reported systems, the solvation of the aggregates by water does not lead to strong changes in the aggregates at the molecular level, since the shape of the IR, UV and CD spectra remain the same, but only change in intensity. Upon further heating from 60 to 80 °C, the APhePyTA aggregates are destabilized and the scattering and CD intensities decrease as the result of the depolymerization of APhePyTA.

The combined VT-CD and UV, IR and scattering results show that water is acting as a chain capper for the supramolecular aggregates and thereby decreases the length of the supramolecular polymers at low temperature and high humidity. A similar effect was also observed for porphyrin-based, supramolecular polymers, in which complexation of water at helix macrodipoles at the polymer chain ends reinforces the binding of the additives to the chain end of the polymer, leading to a decrease in length that is not directly observable by spectroscopy.44

The combined SAXS, VCD, CD and SLS results provide us with key leads to propose a molecular picture of the aggregation behaviour of (S)-PhePyTA. We hypothesize that water assembles at the polymer–solvent interface and thereby subtly changes the polarity of the environment of the (S)-PhePyTA supramolecular polymer. The presence of water stabilizes the dipoles of the electron-poor (S)-PhePyTA core that would otherwise not be stabilized. As a result of this stabilization, the aggregates break up and decrease their size. Concurrently, the increased degrees of freedom in the smaller particles allow the molecules to organize better, leading to an increase of the intensity of the CD spectrum at low temperatures and high-water contents. Thus, the combination of spectroscopy and scattering results reveal that water decreases the size and disorder of the supramolecular aggregates of (S)-PhePyTA, while the morphology in the aggregates remain relatively unchanged.

BiPyTA assembly is dominated by kinetic traps

We next investigated (S)-BiPyTA, the bipyridyl analogue of (S)-BPTA (Fig. 1); a biaryl with an even lower electron density in the aromatic core. The bulk properties of (S)-BiPyTA are completely different from those of its PhePyTA analogues. DSC traces show a melting temperature around 165 °C while SAXS and POM analyses show the presence of crystalline, columnar rectangular mesophases that are stable up to at least 125 °C (Fig. S1–S3). Similarly, VT-IR measurements in the bulk indicate the presence of a hydrogen-bonded amide, which is disrupted around 165 °C (Fig. S4). These results show, in contrast to the amorphous bulk morphology of (S)-PhePyTA, that the bipyridine core with its four amides directs the bulk organization of (S)-BiPyTA into ordered, crystallization-driven structures (Fig. S13).

The study of the self-assembly of (S)-BiPyTA in solution was considerably impaired by its low solubility in alkanes, such as MCH, heptane and decalin. Saturated solutions, which contain approximately 20 μM (S)-BiPyTA, readily precipitated at low temperatures, making solution-state SAXS, IR and SLS measurements as well as VT-CD and UV spectroscopy difficult. The UV spectrum of 15 μM (S)-BiPyTA solutions in dry MCH at 85 °C displays a CD-silent absorption maximum at 228 nm with a shoulder around 295 nm (Fig. 5a). Upon cooling, a very weak CD spectrum emerges, displaying a slightly positive peak around 300 nm and a slightly negative peak below 265 nm. In ambient MCH, a more intense, but highly irreproducible CD spectrum was obtained (Fig. 5b). This indicates a better solubility of the compound in the presence of water in MCH, but the irreproducibility also illustrates the presence of kinetic traps in the (S)-BiPyTA assembly process. The trapping of (S)-BiPyTA in dry and ambient MCH was also apparent in the VT-CD traces that show trends in hysteresis typically observed for kinetically trapped states (Fig. 5c).65 Unfortunately, slower cooling did not resolve the kinetic trapping and the formation of stable and ordered supramolecular polymers was impossible (Fig. S14). (S)-BiPyTA appears to have a strong tendency to crystallize. Nonetheless, as was also observed for an insoluble achiral derivative of (S)-BPTA, in which the chiral alkyl tails were substituted by a linear octyl tail, the insolubility of the pure compound does not preclude coassembly with other compounds to form supramolecular copolymers.53


image file: d1sc03974a-f5.tif
Fig. 5 VT-CD (top panels) and VT-UV (bottom panels) spectra of 15 μM solutions of (S)-BiPyTA in MCH containing 10 (a) and 23 (b) ppm water. The spectra were collected with a cooling rate of 1 °C min−1 at 5 °C intervals, with the red spectra recorded at 85 °C and the blue spectra at 5 °C. The grayscale indicates the temperature gradient from high (light) to low (dark) temperature. (c) VT-CD traces of 15 μM solutions of (S)-BiPyTA in ambient (red traces) and dry (green traces) MCH upon cooling (dark shades) and subsequent heating (light shades).

Copolymerizations

Although both (S)-PhePyTA and (S)-BiPyTA have a low tendency to form ordered helical supramolecular polymers of considerable length, the electron-poor nature of their aromatic cores may drive copolymerization with (S)-BPTA. The latter polymerizes at concentrations as low as 10 μM and remains soluble up to mM concentrations.51 As such, the poorly polymerizing additives may modulate the morphology of the (S)-BPTA copolymers. The copolymerizations were conducted in dry solvents to exclude interference from water, which can considerably hinder copolymer analyses.51 To this end, we first investigated the effect of phenylpyridine derivative (S)-PhePyTA as an additive to the polymerization of (S)-BPTA.

(S)-PhePyTA modulates the length of (S)-BPTA-based polymers

VT-CD and UV measurements on 30 μM samples containing various ratios of (S)-BPTA and (S)-PhePyTA all showed a CD-silent UV maximum at 227 nm above 80 °C (Fig. 6a and S15). Upon cooling below 80 °C, a CD spectrum reminiscent of water-free homopolymers of (S)-BPTA emerges, showing a maximum at 258 nm. Further cooling does not lead to considerable changes in the spectrum, except for the amplitude. Solutions containing low fractions (between 0 and 10 mol%) of (S)-PhePyTA additive show no significant hysteresis and an elongation temperature around 81 °C is observed (Fig. 6b, top panel and S16). Upon further cooling the CD intensities observed for solutions of copolymers containing up to 10 mol% (S)-PhePyTA reach a maximum between approximately 20 and 40 °C. Below this temperature, the intensity gradually decreases, indicating that the helical organization in the polymers weakens or less monomers are polymerized. In contrast, for solutions containing more than 10 mol% (S)-PhePyTA, the elongation temperature increasingly shifts to lower temperature, while the maximum CD intensity decreases considerably. For samples that contain an (S)-PhePyTA mole fraction of 40 mol% or more, hardly any ordered polymers are formed, while the absorption spectra at room temperature retain a relatively low intensity. As no scattering in the UV spectrum at higher wavelengths is observed (Fig. S15), the low absorbance most likely indicates that the biaryl monomers are not molecularly dissolved but are aggregated in a CD-silent aggregate.
image file: d1sc03974a-f6.tif
Fig. 6 (a) Spectra of a sample containing 24 μM (S)-BPTA and 6 μM (S)-PhePyTA in dry MCH. The spectra were recorded at 5 °C intervals with the red, green and blue spectra collected at 95, 40 and 5 °C. Spectra are colour coded on a grayscale going from light (95 °C) to dark (5 °C). (b) Top panel: VT-CD traces of samples containing various ratios of (S)-BPTA and (S)-PhePyTA at a total concentration of 30 μM (blue traces) and a 24 μM sample of (S)-BPTA (yellow trace) in MCH containing less than 10 ppm H2O. Bottom panel: experimental (symbols) and fitted (lines) VT-CD traces of 30 μM mixtures of (S)-BPTA and (S)-PhePyTA in dry MCH. (c) SLS-derived lengths of the (S)-BPTA:(S)-PhePyTA copolymers in MCH containing less than 10 ppm H2O upon addition of varying amounts of (S)-PhePyTA at a fixed (S)-BPTA concentration of 100 μM.

A comparison of solutions containing 30 μM biaryl-based mixtures consisting of 80 mol% (S)-BPTA and 20 mol% (S)-PhePyTA with solutions containing only 24 μM (S)-BPTA sheds further light on the role of the phenylpyridine additive. The latter solution shows an elongation temperature of 80 °C and has a CD intensity of 53 mdeg, in line with our previous report.51 The 30 μM copolymer solution, which also contains 24 μM (S)-BPTA shows, however, an elongation temperature of approximately 78 °C and reaches a maximum CD value of only 34 mdeg around 40 °C. With the van't Hoff equation and the thermodynamic parameters of the (S)-BPTA polymerization, we calculate that (S)-BPTA homopolymers elongate at 78 °C at a monomer concentration of 20 μM. This concentration is very close to the excess of (S)-BPTA in the copolymerization, strongly suggesting that (S)-PhePyTA sequesters (S)-BPTA from the polymerization in an equimolar ratio. This role of (S)-PhePyTA as a sequestrator explains the VT-CD of all samples containing up to 30 mol% of (S)-PhePyTA (Fig. 6b), which further corroborates the equimolar sequestration of (S)-BPTA by (S)-PhePyTA.

Additional thermodynamic insight into the sequestration of (S)-BPTA by (S)-PhePyTA was obtained by fitting a mass-balance model that describes the respective homopolymerization and sequestration to the VT-CD traces (full details in the ESI). The fits of the mixtures containing up to 30 mol% (S)-PhePyTA are in good agreement with the experimental data (Fig. 6b, lower panel). From the fits, upper and lower bounds on the value of the enthalpy and entropy of the sequestration event are obtained. The model is in good agreement with the data for several sets of thermodynamic values with enthalpy values between −80 and −107 kJ mol−1 and entropy values between −89 and −169 J mol−1 K−1, (Fig. S17). Unfortunately, the model is not able to give clear indications on enthalpic differences between the respective homo- and hetero-interactions between (S)-BPTA and (S)-PhePyTA. However, the upper bound for the entropic penalty of −169 J mol−1 K−1 indicates that the entropic penalty of the hetero-interaction is less than the entropic penalty of ordering the monomers in the homopolymers, suggesting that the sequestered complex is rather disorganized. This disorganized nature of the sequestered species is in agreement with the lack of a strong CD signal. Interestingly, when we tried to fit the entire dataset, which includes the VT-CD traces of samples containing 40, 50 and 60 mol% (S)-PhePyTA, the model incorrectly predicts an elongation of (S)-BPTA at low temperatures, rather than around 60 °C (Fig. S18). The model's lower elongation temperatures indicate that at higher (S)-PhePyTA ratios and low temperatures, there may be a sufficiently large thermodynamic driving force for (S)-PhePyTA to act as an intercalator or chain capping agent. Thus, while (S)-PhePyTA may act as chain capper or intercalator at low temperatures, the VT-CD results show that, at 60 °C, the phenylpyridine-based additive acts primarily as a sequestrator of (S)-BPTA.

To confirm the role of an additive in supramolecular copolymerizations, spectroscopic studies were complemented by scattering techniques to reveal information on the size of the copolymers.23 To this end, we conducted multi-angle SLS measurements at 30, 45 and 60 °C on dry MCH solutions containing 100 μM (S)-BPTA and varying amounts of (S)-PhePyTA (Fig. 6c). After fitting the scattering results to a cylindrical model, the experiments show that at all temperatures the length of the supramolecular polymers gradually decreases as the phenylpyridine additive is added. This gradual decrease in polymer length upon addition of (S)-PhePyTA is a hallmark of the sequestrating role of (S)-PhePyTA. In contrast, a sharp decrease would be indicative of a chain capper, whereas a subtle length increase would indicate copolymerizing or intercalating additives.23 Furthermore, when more than 10 mol% (S)-PhePyTA is present in the system, the slope of the scattering profiles decreases at high q-values (Fig. S19–S21). This change in slope suggests the presence of a second population of non-cylindrical aggregates next to the cylindrical supramolecular polymers, further corroborating the predominantly sequestrating role of (S)-PhePyTA. Surprisingly, the phenylpyridine core of the (S)-PhePyTA does not lead to the efficient formation of copolymers with (S)-BPTA. Rather, the phenylpyridyl core directs the formation of small, sequestrating dimers or oligomers through which the chain length of the (S)-BPTA polymers can be tuned in a controlled manner.

(S)-BiPyTA modulates (S)-BPTA-based polymers as a function of temperature

Next, we investigated the role of (S)-BiPyTA in the polymerization of (S)-BPTA using an identical approach as employed for (S)-PhePyTA. The VT-UV and CD spectra show that the absorption spectra gradually change upon increasing the molar fraction of (S)-BiPyTA in 30 μM solutions of (S)-BPTA and (S)-BiPyTA. The VT-CD spectra for all copolymerizations show identical spectral shapes, which indicates that the microscopic structure of the ordered aggregates present in solution remains identical to the structure of the (S)-BPTA homopolymers (Fig. 7a and S22). The VT-CD intensity at 258 nm shows that at 30 μM total monomer concentration, the copolymers containing up to 30 mol% of (S)-BiPyTA all elongate at 81 °C and minimal hysteresis and water dependency is observed (Fig. 7b, S23 and S24). Together with the CD intensities around the elongation temperature, which are similar to (S)-BPTA homopolymers, these results show that (S)-BiPyTA readily copolymerizes with (S)-BPTA. When the temperature is further decreased, the CD intensity reaches a maximum, which occurs at higher temperatures for higher molar ratios of (S)-BiPyTA in the copolymers. After reaching a maximum, the CD intensity gradually decreases as the temperature is further decreased and solutions containing 20 mol% or more (S)-BiPyTA do not show any CD intensity at 20 °C anymore. For solutions containing more than 30 mol% (S)-BiPyTA, the elongation temperatures become increasingly lower, while solutions containing 60 mol% do not show any considerable formation of supramolecular polymers at all. In contrast to the results obtained for (S)-PhePyTA, the VT-CD traces of the (S)-BPTA:(S)-BiPyTA solutions suggest that (S)-BiPyTA copolymerizes with (S)-BPTA at high temperatures, while at low temperatures a similar destabilization of the polymers occurs as observed for (S)-PhePyTA.

The incorporation of small fractions of (S)-BiPyTA into supramolecular polymers of (S)-BPTA at high temperatures is corroborated by SLS measurements. At 60 °C, the supramolecular polymers do not show a noticeable decrease in polymer length when (S)-BiPyTA is added to 100 μM solutions of (S)-BPTA (Fig. 7c). In addition, the scattering profiles of the samples at 60 °C containing (S)-BiPyTA fractions can be described with a single cylindrical model (Fig. S25), suggesting that only a single polymer species is present. Together with the spectroscopic data, this result points to a predominant intercalating role of (S)-BiPyTA in which the additive readily incorporates into the (S)-BPTA-based polymers at temperatures of 60 °C. However, due to destabilizing dipolar interactions, (S)-BiPyTA does not form contacts with other (S)-BiPyTA monomers, and this results in only a modest decrease in polymer length at low additive ratios. At lower temperatures, where the CD intensity of the (S)-BPTA:(S)-BiPyTA mixtures decreases, SLS shows a gradual decrease in the polymer length, while the scattering profiles of samples containing 10 mol% (S)-BiPyTA or more show a change in slope at high q-values (Fig. 7c, S26 and S27), indicating that other aggregates are formed. Thus, the SLS results confirm that at low temperatures, (S)-BiPyTA most likely functions as a sequestrator of (S)-BPTA.


image file: d1sc03974a-f7.tif
Fig. 7 (a) Spectra of a sample containing 24 μM (S)-BPTA and 6 μM (S)-BiPyTA in dry MCH. The spectra were recorded at 5 °C intervals with the red, green and blue spectra collected at 95, 40 and 5 °C. Spectra are colour coded on a grayscale going from light (95 °C) to dark (5 °C). (b) Top panel: VT-CD traces of samples containing various ratios of (S)-BPTA and (S)-BiPyTA at a total concentration of 30 μM (blue traces) and a 24 μM sample of (S)-BPTA (yellow trace) in MCH containing less than 10 ppm H2O. Bottom panel: VT-CD traces of MCH solutions containing 15 μM (S)-BPTA, and 15 μM of both (S)-BPTA and 4,4′-bipydirine. (c) SLS-derived lengths of the (S)-BPTA:(S)-BiPyTA copolymers in MCH containing less than 10 ppm H2O upon addition of varying amounts of (S)-BiPyTA at a fixed (S)-BPTA concentration of 100 μM.

To gain a more detailed insight into the driving forces leading to copolymerization of (S)-BiPyTA with (S)-BPTA at higher temperatures, we also studied a solution containing 15 μM (S)-BPTA and 15 μM 4,4′-bipyridine (Fig. 7b, lower panel). The 4,4′-bipyridine additive features a similar electron-poor aromatic core but does not possess the ability to form intermolecular hydrogen bonds with the amides of (S)-BPTA. When comparing the VT-CD traces of this mixture with the VT-CD trace of a 15 μM (S)-BPTA homopolymerization, no significant differences can be observed apart from changes in intensity that are due to different levels of humidity in the solution. Thus, dipolar interactions alone are not sufficient for the intercalation into the (S)-BPTA-based polymers. Instead, the hydrogen-bonding ability of the additive appears key to further drive the incorporation of (S)-BiPyTA into the polymers. As such, we conclude that the subtle changes in hydrogen bonding interactions and dipolar character of the (S)-PhePyTA and (S)-BiPyTA additives can lead to profound changes in supramolecular behaviour (Fig. 8).


image file: d1sc03974a-f8.tif
Fig. 8 Cartoon representation of the aggregation behaviour of (S)-PhePyTA and (S)-BiPyTA in the absence and presence of (S)-BPTA.

Conclusions

In this work, we have studied the supramolecular aggregation in methylcyclohexane (MCH) of phenylpyridine- and bipyridine-based analogues of the previously studied biphenyltetracarboxamide (S)-BPTA. Unlike the long and ordered supramolecular polymers formed by (S)-BPTA, the phenylpyridine (S)-PhePyTA forms short, disorganized fibers, while the bipyridine (S)-BiPyTA forms kinetically trapped, ill-defined supramolecular aggregates. With a combination of spectroscopic and scattering techniques, it was found that water controls the chain length of the (S)-PhePyTA aggregates in ambient MCH and is responsible for the small size of these aggregates. With the decreasing solubility and ordering in the supramolecular polymerization upon increasing the electron deficiency of the aromatic core, the biaryl monomers highlight the balance between solubility and aggregation driving force that is required to form ordered supramolecular polymers.

Although the pyridine-based molecules do not form long, ordered supramolecular polymers by themselves, copolymerization experiments show that they can be used to control the length and stability of (S)-BPTA-based polymers. By sequestrating (S)-BPTA monomers at high temperatures, (S)-PhePyTA suppresses the length and elongation temperature of (S)-BPTA homopolymers. At lower temperatures, the weak decrease of the polymer length suggests that the additive further destabilizes the polymers through intercalation. In contrast, (S)-BiPyTA intercalates into the polymers already at high temperatures, giving subtle control over the length of the (S)-BPTA-based copolymers.

These observations illustrate the delicate energetic balances encountered in these systems, as was also observed for other biphenyl systems.51 With this, we provide further insights into the dramatic effects that small structural variations can have on supramolecular systems. To gain a further understanding of these phenomena, a combination of thorough experimental and computational analyses is crucial. We envision that such systematic studies will lead to further control over supramolecular materials for a wide range of biomedical and opto-electronical applications. By acting as synthetic analogues of biochemical chaperones, such additive molecules are thereby a valuable tool in the expanding toolbox of non-covalent synthesis.

Data availability

All relevant data is presented in the paper and ESI. Raw data is available upon request by email to E. W. M. The Matlab code used for fitting the mass-balance model can be found at https://www.github.com/mathijs-m/BPTA_polymerization_sequestration.

Author contributions

E. W. M. and T. I. devised the project. M. F. J. M. and T. I. developed the research and performed the majority of the experiments and writing. M. F. J. M. carried out all the calculations. M. A. J. K. analyzed the stacking fashion of PhePyTA aggregates via DFT calculation and VCD experiments. B. A. G. L. measured X-ray diffraction and DSC. E. W. collected VT-IR spectra. L. N. J. W. performed SAXS experiment. All authors have given approval to the final version of the manuscript.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

We acknowledge Dr Rodrigo Magaña Rodriguez for fruitful discussions. We thank Dr Marcin Ślęczkowski for providing the (S)-chiral amine starting material and help during NMR experiments. This work received financially supported by The Netherlands Organization for Scientific Research (TOP-PUNT grant 10018944, ECHO grant 713.016.003) and the Dutch Ministry of Education, Culture and Science (Gravity program FMS 024.001.035). The authors are grateful for the financial support from Kao corporation.

Notes and references

  1. W. A. Braunecker and K. Matyjaszewski, Controlled/Living Radical Polymerization: Features, Developments, and Perspectives, Prog. Polym. Sci., 2007, 32(1), 93–146 CrossRef CAS.
  2. G. Moad, E. Rizzardo and S. H. Thang, Radical Addition–fragmentation Chemistry in Polymer Synthesis, Polymer, 2008, 49(5), 1079–1131 CrossRef CAS.
  3. J. Nicolas, Y. Guillaneuf, C. Lefay, D. Bertin, D. Gigmes and B. Charleux, Nitroxide-Mediated Polymerization, Prog. Polym. Sci., 2013, 38(1), 63–235 CrossRef CAS.
  4. M. Rahman and C. S. Brazel, The Plasticizer Market: An Assessment of Traditional Plasticizers and Research Trends to Meet New Challenges, Prog. Polym. Sci., 2004, 29(12), 1223–1248 CrossRef CAS.
  5. M. G. A. Vieira, M. A. da Silva, L. O. dos Santos and M. M. Beppu, Natural-Based Plasticizers and Biopolymer Films: A Review, Eur. Polym. J., 2011, 47(3), 254–263 CrossRef CAS.
  6. T. Mekonnen, P. Mussone, H. Khalil and D. Bressler, Progress in Bio-Based Plastics and Plasticizing Modifications, J. Mater. Chem. A, 2013, 1(43), 13379–13398 RSC.
  7. D. L. Rabenstein, Heparin and Heparan Sulfate: Structure and Function, Nat. Prod. Rep., 2002, 19(3), 312–331 RSC.
  8. B. P. Toole, Hyaluronan: From Extracellular Glue to Pericellular Cue, Nat. Rev. Cancer, 2004, 4(7), 528–539 CrossRef CAS PubMed.
  9. F. Zhang, Z. Zhang and R. J. LinhardtGlycosaminoglycans, in Handbook of Glycomics, ed. R. D. Cummings and J. M. Pierce, Elsevier, 2010, pp. 59–80 Search PubMed.
  10. N. A. Ayoub, J. E. Garb, R. M. Tinghitella, M. A. Collin and C. Y. Hayashi, Blueprint for a High-Performance Biomaterial: Full-Length Spider Dragline Silk Genes, PLoS One, 2007, 2(6), e514 CrossRef PubMed.
  11. J. A. Kluge, O. Rabotyagova, G. G. Leisk and D. L. Kaplan, Spider Silks and Their Applications, Trends Biotechnol., 2008, 26(5), 244–251 CrossRef CAS PubMed.
  12. A. D. Malay, K. Arakawa and K. Numata, Analysis of Repetitive Amino Acid Motifs Reveals the Essential Features of Spider Dragline Silk Proteins, PLoS One, 2017, 12(8), e0183397 CrossRef PubMed.
  13. T. Aida, A. Takemura, M. Fuse and S. Inoue, Synthesis of a Novel Amphiphilic Porphyrin Carrying Water-Soluble Polyether Side Chains of Controlled Chain Length. Formation of a Cofacial Molecular Assembly in Aqueous Media, J. Chem. Soc., Chem. Commun., 1988, 5, 391–393 RSC.
  14. Q. Wang, J. L. Mynar, M. Yoshida, E. Lee, M. Lee, K. Okuro, K. Kinbara and T. Aida, High-Water-Content Mouldable Hydrogels by Mixing Clay and a Dendritic Molecular Binder, Nature, 2010, 463(7279), 339–343 CrossRef CAS PubMed.
  15. Y. Yanagisawa, Y. Nan, K. Okuro and T. Aida, Mechanically Robust, Readily Repairable Polymers via Tailored Noncovalent Cross-linking, Science, 2018, 359(6371), 72–76 CrossRef CAS PubMed.
  16. G. A. Silva, C. Czeisler, K. L. Niece, E. Beniash, D. A. Harrington, J. A. Kessler and S. I. Stupp, Selective Differentiation of Neural Progenitor Cells by High-Epitope Density Nanofibers, Science, 2004, 303(5662), 1352–1355 CrossRef CAS PubMed.
  17. Z. Huang, C. J. Newcomb, P. Bringas, S. I. Stupp and M. L. Snead, Biological Synthesis of Tooth Enamel Instructed by an Artificial Matrix, Biomaterials, 2010, 31(35), 9202–9211 CrossRef CAS PubMed.
  18. Z. Yu, F. Tantakitti, T. Yu, L. C. Palmer, G. C. Schatz and S. I. Stupp, Simultaneous Covalent and Noncovalent Hybrid Polymerizations, Science, 2016, 351(6272), 497–502 CrossRef CAS PubMed.
  19. T. Aida, E. W. Meijer and S. I. Stupp, Functional Supramolecular Polymers, Science, 2012, 335(6070), 813–817 CrossRef CAS PubMed.
  20. M. J. Webber, E. A. Appel, E. W. Meijer and R. Langer, Supramolecular Biomaterials, Nat. Mater., 2016, 15(1), 13–26 CrossRef CAS.
  21. O. J. G. M. Goor, S. I. S. Hendrikse, P. Y. W. Dankers and E. W. Meijer, From Supramolecular Polymers to Multi-Component Biomaterials, Chem. Soc. Rev., 2017, 46(21), 6621–6637 RSC.
  22. B. Adelizzi, N. J. J. Van Zee, L. N. J. N. J. de Windt, A. R. A. R. A. Palmans and E. W. W. Meijer, Future of Supramolecular Copolymers Unveiled by Reflecting on Covalent Copolymerization, J. Am. Chem. Soc., 2019, 141(15), 6110–6121 CrossRef CAS.
  23. E. Weyandt, M. F. J. Mabesoone, L. N. J. de Windt, E. W. Meijer, A. R. A. Palmans and G. Vantomme, How to Determine the Role of an Additive on the Length of Supramolecular Polymers?, Organic Materials, 2020, 02(02), 129–142 CrossRef CAS.
  24. M. M. J. Smulders, A. P. H. J. Schenning and E. W. Meijer, Insight into the Mechanisms of Cooperative Self-Assembly: The “Sergeants-and-Soldiers” Principle of Chiral and Achiral C3-Symmetrical Discotic Triamides, J. Am. Chem. Soc., 2008, 130(2), 606–611 CrossRef CAS.
  25. T. E. Kaiser, V. Stepanenko and F. Würthner, Fluorescent J-Aggregates of Core-Substituted Perylene Bisimides: Studies on Structure−Property Relationship, Nucleation−Elongation Mechanism, and Sergeants-and-Soldiers Principle, J. Am. Chem. Soc., 2009, 131(19), 6719–6732 CrossRef CAS PubMed.
  26. M. Liu, L. Zhang and T. Wang, Supramolecular Chirality in Self-Assembled Systems, Chem. Rev., 2015, 115(15), 7304–7397 CrossRef CAS PubMed.
  27. J. van Gestel, A. R. A. Palmans, B. Titulaer, J. A. J. M. Vekemans and E. W. Meijer, “Majority-Rules” Operative in Chiral Columnar Stacks of C3-Symmetrical Molecules, J. Am. Chem. Soc., 2005, 127(15), 5490–5494 CrossRef CAS PubMed.
  28. W. Jin, T. Fukushima, M. Niki, A. Kosaka, N. Ishii and T. Aida, Self-Assembled Graphitic Nanotubes with One-Handed Helical Arrays of a Chiral Amphiphilic Molecular Graphene, Proc. Natl. Acad. Sci. U. S. A., 2005, 102(31), 10801–10806 CrossRef CAS PubMed.
  29. M. M. J. Smulders, P. J. M. Stals, T. Mes, T. F. E. Paffen, A. P. H. J. Schenning, A. R. A. Palmans and E. W. Meijer, Probing the Limits of the Majority-Rules Principle in a Dynamic Supramolecular Polymer, J. Am. Chem. Soc., 2010, 132(2), 620–626 CrossRef CAS.
  30. Y. Dorca, E. E. Greciano, J. S. Valera, R. Gómez and L. Sánchez, Hierarchy of Asymmetry in Chiral Supramolecular Polymers: Toward Functional, Helical Supramolecular Structures, Chem.–Eur. J., 2019, 25(23), 5848–5864 CrossRef CAS.
  31. A. Das, G. Vantomme, A. J. Markvoort, H. M. M. Ten Eikelder, M. Garcia-Iglesias, A. R. A. Palmans and E. W. Meijer, Supramolecular Copolymers: Structure and Composition Revealed by Theoretical Modeling, J. Am. Chem. Soc., 2017, 139(20), 7036–7044 CrossRef CAS.
  32. B. Adelizzi, A. Aloi, A. J. Markvoort, H. M. M. Ten Eikelder, I. K. Voets, A. R. A. Palmans and E. W. Meijer, Supramolecular Block Copolymers under Thermodynamic Control, J. Am. Chem. Soc., 2018, 140(23), 7168–7175 CrossRef CAS PubMed.
  33. M. Wehner, M. I. S. Röhr, M. Bühler, V. Stepanenko, W. Wagner and F. Würthner, Supramolecular Polymorphism in One-Dimensional Self-Assembly by Kinetic Pathway Control, J. Am. Chem. Soc., 2019, 141(14), 6092–6107 CrossRef CAS PubMed.
  34. A. Sarkar, T. Behera, R. Sasmal, R. Capelli, C. Empereur-mot, J. Mahato, S. S. Agasti, G. M. Pavan, A. Chowdhury and S. J. George, Cooperative Supramolecular Block Copolymerization for the Synthesis of Functional Axial Organic Heterostructures, J. Am. Chem. Soc., 2020, 142(26), 11528–11539 CrossRef CAS PubMed.
  35. R. van Buel, D. Spitzer, C. M. Berac, P. van der Schoot, P. Besenius and S. Jabbari-Farouji, Supramolecular Copolymers Predominated by Alternating Order: Theory and Application, J. Chem. Phys., 2019, 151(1), 014902 CrossRef PubMed.
  36. A. Sarkar, R. Sasmal, C. Empereur-mot, D. Bochicchio, S. V. K. Kompella, K. Sharma, S. Dhiman, B. Sundaram, S. S. Agasti, G. M. Pavan and S. J. George, Self-Sorted, Random, and Block Supramolecular Copolymers via Sequence Controlled, Multicomponent Self-Assembly, J. Am. Chem. Soc., 2020, 142(16), 7606–7617 CrossRef CAS PubMed.
  37. H. M. M. ten Eikelder, B. Adelizzi, A. R. A. Palmans and A. J. Markvoort, Equilibrium Model for Supramolecular Copolymerizations, J. Phys. Chem. B, 2019, 123(30), 6627–6642 CrossRef CAS.
  38. D. Bochicchio, M. Salvalaglio and G. M. Pavan, Into the Dynamics of a Supramolecular Polymer at Submolecular Resolution, Nat. Commun., 2017, 8(1), 147 CrossRef.
  39. D. Bochicchio and G. M. Pavan, Molecular Modelling of Supramolecular Polymers, Adv. Phys.: X, 2018, 3(1), 1436408 Search PubMed.
  40. F. Helmich, C. C. Lee, M. M. L. Nieuwenhuizen, J. C. Gielen, P. C. M. Christianen, A. Larsen, G. Fytas, P. E. L. G. Leclère, A. P. H. J. Schenning and E. W. Meijer, Dilution-Induced Self-Assembly of Porphyrin Aggregates: A Consequence of Coupled Equilibria, Angew. Chem., Int. Ed., 2010, 49(23), 3939–3942 CrossRef CAS.
  41. S.-G. Chen, Y. Yu, X. Zhao, Y. Ma, X.-K. Jiang and Z.-T. Li, Highly Stable Chiral (A) 6 –B Supramolecular Copolymers: A Multivalency-Based Self-Assembly Process, J. Am. Chem. Soc., 2011, 133(29), 11124–11127 CrossRef CAS PubMed.
  42. T. Hirose, F. Helmich and E. W. Meijer, Photocontrol over Cooperative Porphyrin Self-Assembly with Phenylazopyridine Ligands, Angew. Chem., Int. Ed., 2013, 52(1), 304–309 CrossRef CAS PubMed.
  43. S. H. Jung, D. Bochicchio, G. M. Pavan, M. Takeuchi and K. Sugiyasu, A Block Supramolecular Polymer and Its Kinetically Enhanced Stability, J. Am. Chem. Soc., 2018, 140(33), 10570–10577 CrossRef CAS PubMed.
  44. M. F. J. Mabesoone, G. M. ter Huurne, A. R. A. Palmans and E. W. Meijer, How Water in Aliphatic Solvents Directs the Interference of Chemical Reactivity in a Supramolecular System, J. Am. Chem. Soc., 2020, 142(28), 12400–12408 CrossRef CAS PubMed.
  45. W. Knoben, N. A. M. Besseling, L. Bouteiller and M. A. Cohen Stuart, Dynamics of Reversible Supramolecular Polymers: Independent Determination of the Dependence of Linear Viscoelasticity on Concentration and Chain Length by Using Chain Stoppers, Phys. Chem. Chem. Phys., 2005, 7(11), 2390–2398 RSC.
  46. O. Colombani, C. Barioz, L. Bouteiller, C. Chanéac, L. Fompérie, F. Lortie and H. Montés, Attempt toward 1D Cross-Linked Thermoplastic Elastomers: Structure and Mechanical Properties of a New System, Macromolecules, 2005, 38(5), 1752–1759 CrossRef CAS.
  47. W. Knoben, N. A. M. M. Besseling and M. A. Cohen Stuart, Chain Stoppers in Reversible Supramolecular Polymer Solutions Studied by Static and Dynamic Light Scattering and Osmometry, Macromolecules, 2006, 39(7), 2643–2653 CrossRef CAS.
  48. W. Knoben, N. A. M. Besseling and M. A. Cohen Stuart, Direct Measurement of Depletion and Hydrodynamic Forces in Solutions of a Reversible Supramolecular Polymer, Langmuir, 2007, 23(11), 6095–6105 CrossRef CAS PubMed.
  49. T. Pinault, C. Cannizzo, B. Andrioletti, G. Ducouret, F. F. Lequeux and L. Bouteiller, Anions as Efficient Chain Stoppers for Hydrogen-Bonded Supramolecular Polymers, Langmuir, 2009, 25(15), 8404–8407 CrossRef CAS PubMed.
  50. G. M. ter Huurne, P. Chidchob, A. Long, A. Martinez, A. R. A. Palmans and G. Vantomme, Controlling the Length of Cooperative Supramolecular Polymers with Chain Cappers, Chem.–Eur. J., 2020, 26(44), 9964–9970 CrossRef CAS PubMed.
  51. N. J. Van Zee, B. Adelizzi, M. F. J. Mabesoone, X. Meng, A. Aloi, R. H. Zha, M. Lutz, I. A. W. Filot, A. R. A. Palmans and E. W. Meijer, Potential Enthalpic Energy of Water in Oils Exploited to Control Supramolecular Structure, Nature, 2018, 558(7708), 100–103 CrossRef CAS PubMed.
  52. R. Wolfenden and A. Radzicka, On the Probability of Finding a Water Molecule in a Nonpolar Cavity, Science, 1994, 265(5174), 936–937 CrossRef CAS PubMed.
  53. N. J. Van Zee, M. F. J. Mabesoone, B. Adelizzi, A. R. A. Palmans and E. W. Meijer, Biasing the Screw-Sense of Supramolecular Coassemblies Featuring Multiple Helical States, J. Am. Chem. Soc., 2020, 142(47), 20191–20200 CrossRef CAS PubMed.
  54. R. van der Weegen, P. A. Korevaar, P. Voudouris, I. K. Voets, T. F. A. de Greef, J. A. J. M. Vekemans and E. W. Meijer, Small Sized Perylene-Bisimide Assemblies Controlled by Both Cooperative and Anti-Cooperative Assembly Processes, Chem. Commun., 2013, 49(49), 5532 RSC.
  55. M. M. J. Smulders, T. Buffeteau, D. Cavagnat, M. Wolffs, A. P. H. J. Schenning and E. W. Meijer, C 3-Symmetrical Self-Assembled Structures Investigated by Vibrational Circular Dichroism, Chirality, 2008, 20(9), 1016–1022 CrossRef CAS PubMed.
  56. B. Nieto-Ortega, F. García, G. Longhi, E. Castiglioni, J. Calbo, S. Abbate, J. T. López Navarrete, F. J. Ramírez, E. Ortí, L. Sánchez and J. Casado, On the Handedness of Helical Aggregates of C3 Tricarboxamides: A Multichiroptical Characterization, Chem. Commun., 2015, 51(48), 9781–9784 RSC.
  57. J. S. Valera, R. Sánchez-Naya, F. J. Ramírez, J. L. Zafra, R. Gómez, J. Casado and L. Sánchez, Solvent-Directed Helical Stereomutation Discloses Pathway Complexity on N-Heterotriangulene-Based Organogelators, Chem.–Eur. J., 2017, 23(46), 11141–11146 CrossRef CAS PubMed.
  58. M. A. J. Koenis, A. Osypenko, G. Fuks, N. Giuseppone, V. P. Nicu, L. Visscher and W. J. Buma, Self-Assembly of Supramolecular Polymers of N-Centered Triarylamine Trisamides in the Light of Circular Dichroism: Reaching Consensus between Electrons and Nuclei, J. Am. Chem. Soc., 2020, 142(2), 1020–1028 CrossRef CAS PubMed.
  59. D. Görl and F. Würthner, Entropically Driven Self-Assembly of Bolaamphiphilic Perylene Dyes in Water, Angew. Chem., Int. Ed., 2016, 55(39), 12094–12098 CrossRef PubMed.
  60. K. V. Rao, D. Miyajima, A. Nihonyanagi, T. Aida, K. V. Rao, D. Miyajima, A. Nihonyanagi and T. Aida, Thermally Bisignate Supramolecular Polymerization, Nat. Chem., 2017, 9(11), 1133–1139 CrossRef PubMed.
  61. V. Grande, B. Soberats, S. Herbst, V. Stepanenko and F. Würthner, Hydrogen-Bonded Perylene Bisimide J-Aggregate Aqua Material, Chem. Sci., 2018, 9(34), 6904–6911 RSC.
  62. P. P. N. Syamala, B. Soberats, D. Görl, S. Gekle and F. Würthner, Thermodynamic Insights into the Entropically Driven Self-Assembly of Amphiphilic Dyes in Water, Chem. Sci., 2019, 10(40), 9358–9366 RSC.
  63. K. V. Rao, M. F. J. Mabesoone, D. Miyajima, A. Nihonyanagi, E. W. Meijer and T. Aida, Distinct Pathways in “Thermally Bisignate Supramolecular Polymerization”: Spectroscopic and Computational Studies, J. Am. Chem. Soc., 2020, 142(1), 598–605 CrossRef CAS PubMed.
  64. P. P. N. Syamala, F. Würthner and P. N. Syamala, Modulation of the Self-assembly of Π-Amphiphiles in Water from Enthalpy- to Entropy-Driven by Enwrapping Substituents, Chem.–Eur. J., 2020, 26(38), 8426–8434 CrossRef CAS PubMed.
  65. V. R. W. Harkness, N. Avakyan, H. F. Sleiman and A. K. Mittermaier, Mapping the Energy Landscapes of Supramolecular Assembly by Thermal Hysteresis, Nat. Commun., 2018, 9(1), 3152 CrossRef PubMed.

Footnotes

Electronic supplementary information (ESI) available. See DOI: 10.1039/d1sc03974a
Equal contributions.

This journal is © The Royal Society of Chemistry 2021