Open Access Article
Songyang Su‡
a,
Lu Shi‡a,
Wentao Yao‡a,
Yang Wangb,
Peichao Zoua,
Kangwei Liua,
Min Wanga,
Feiyu Kangc and
Cheng Yang
*a
aDivision of Energy and Environment, Tsinghua Shenzhen International Graduate School, Tsinghua University, Shenzhen 518055, China. E-mail: yang.cheng@sz.tsinghua.edu.cn
bState Key Laboratory of Electronic Thin Films and Integrated Devices, School of Optoelectronic Information, University of Electronic Science and Technology of China (UESTC), Chengdu 610054, China
cSchool of Materials Science and Engineering, Tsinghua University, Beijing 100084, China
First published on 28th February 2020
Despite significant advances in cathode materials, developing high-performance anodes remains a key challenge for future pseudocapacitors. Fe2O3 has been considered as a promising anode candidate due to its high theoretical capacitance, environmental benignity, and earth-abundant characteristics. However, the low electronic conductivity and poor cyclability of Fe2O3 significantly limit its practical application. In this work, a 3D nickel-metalized carbon nanofiber network was developed to deposit an Fe2O3 nanosheet anode. The nickel layer not only improved the electronic conductivity and the wettability of the 3D carbon substrate but also benefit the stability of the Fe2O3/carbon interfaces and the stress-release upon cycling. As a result, the newly designed Fe2O3 anode composite exhibited a high areal capacitance of 1.80 F cm−2 at a high mass loading of 4.2 mg cm−1 and ultra-high capacitance retention of 85.1% after successive 100
000 cycles, outperformed most of the reported Fe2O3-based anode materials. Extended the interface metallization method to a MnO2 cathode, excellent capacitance retention of 108.2% was reached after 26
000 cycles, suggesting a potentially broad application of such an interface-management method in elevating the stability of metal oxide materials in various pseudocapacitive energy storage devices.
Among various pseudocapacitive materials, hematite (α-Fe2O3) is considered as a promising anode, because of its earth abundance, minimal environmental impact, high theoretical specific capacitance, and moderate potential window.7–10 Similar to other transitional metal oxides, the electrochemical performance of Fe2O3 is limited by its low electronic conductivity (∼10−14 S cm−1) and poor mechanical strength upon cycling.11–13 To improve the electrochemical performance of Fe2O3, several strategies have been developed. To improve the electronic conductivity, compositing with conductive additives or elemental doping are generally adopted.14–16 Nanostructures can be used to enlarge the accessible surface area.17 Other studies regarding defects-engineering, such as plasma activation, have been demonstrated to be feasible in optimizing the electrochemical activity and electronic conductivity.12 Although many efforts have been devoted, the reported capacitive performances of Fe2O3 based electrodes are still far from ideal, especially the specific capacitance and cycle performance (as far as we know, the record cycle performance of Fe2O3 is 50
000 cycles with the capacitance retention is 95.8%).18 Another concern is that most reported electrochemical performances were based on a limited mass loading level (e.g. <2 mg cm−2), which is far from practical applications.
Recent reports show amorphous materials can provide much better cycle stability than their crystalline counterparts, due to the structural disorder, isotropic nature of ion diffusion, and abundant percolation pathways.19–23 Amorphous materials, such as nickel hydroxide and mixed-metal hydroxide, have been developed as excellent cathode materials for supercapacitors.19,20 As for the anode materials, low-crystalline iron oxide hydroxide also has been developed.21–23 Although lots of efforts have been devoted to the development of hydroxide-based materials for high-performance electrodes, the study of amorphous metal oxide-based anode materials is still quite limited.
Herein, we report a high-performance pseudocapacitive Fe2O3 anode composite, which consists of crystalline-in-amorphous Fe2O3 nanosheets deposited on a three-dimensional (3D) nickel-metalized carbon nanofiber (CNF-Ni). The nickel-metal layer not only improved the electronic conductivity and affinity of the CNF substrate toward Fe2O3 but also greatly enhanced the stability of the interfaces between the active material and the conductive network. The reason may due to the comparative Young's modulus and electronic structure between nickel (207 GPa) and iron (200 GPa),24 which may help improve the mechanical properties of the interfaces. Moreover, the numerous crystalline/amorphous phase interfaces inside the Fe2O3 nanosheets offered isotropic and abundant “highways” for electrons and ions diffusion. Consequently, the CNF-Ni@Fe2O3 anode exhibited a large specific capacitance of 428.6 F g−1, a competitive areal capacitance of 1.80 F cm−2 under a high mass loading of 4.2 mg cm−2, and superior cyclability of 85.1% after cycling for 100
000 times. Adopting the 3D CNF-Ni substrate to load a MnO2 cathode, excellent capacitance retention of 108.2% was reached after 26
000 cycles. Coupling the CNF-Ni@Fe2O3 anode with the CNF-Ni@MnO2 cathode, the assembled asymmetric pseudocapacitor showed a maximum energy density of 4.32 mW h cm−3 and a maximum power density of 514.80 mW cm−3. The superior cycling stability of the Fe2O3 anode and MnO2 cathode demonstrated a possible wide application of our nickel metallization method in elevating the stability of metal oxides in various pseudocapacitive energy storage devices.
000 g mol−1) and Zn(Ac)2 (0.607 g) were mixed in dimethylformamide (10 mL) at 25 °C with intense magnetic stirring for 72 h to obtain the spinning solution. Electrospinning was conducted with a feeding rate of 0.14 mm min−1 through a stainless-steel pipette needle (23 gauge, orifice diameter = 340 μm) under a working potential of 18 kV. PAN nanofibers were collected on a sheet of aluminum foil placed on the roller with a rolling speed of 40 rpm. The distance between the needle and the aluminum foil was 15 cm. The as-obtained PAN nanofibers were stabilized at 290 °C for 1 h in air and were subsequently carbonized at 1100 °C for 2 h in Ar with a heating rate of 5 °C min−1 in an atmosphere of Ar to obtain the carbon nanofiber (designated as CNF). After the carbonization process, the products were washed by acetone and 1 M NaOH solution for 3 times and then dried at 60 °C for 2 h.
The Ni depositing solution was prepared by adding 260 g NiSO4·6H2O, 40 g NiCl2·6H2O, 40 g H3BO3, and 0.2 g C12H25NaO4S into 1 L DI water. After full dissolving, the pH of the solution was adjusted to 4.8 by NH3·H2O (28 wt%). Then, a piece of CNF was used as the working electrode, nickel foam was used as the counter electrode and a saturated calomel electrode (SCE) was used as the reference electrode for electrodeposition of Ni, at a constant current density of −25 mA cm−2 for 2 h, the nickel-coated carbon nanofiber (designated as CNF-Ni) can be obtained.
Cyclic voltammetry (CV), galvanostatic discharging (GD), galvanostatic charging/discharging (GCD), and electrochemical impedance spectroscopy (EIS) of the as-prepared samples were investigated on an electrochemical station (VMP3, Bio-Logic, France). The mass-specific capacitance (Cm), areal specific capacitance (Ca), volume-specific energy density (Ev), and volume power density (Pv) were calculated from the CV or GCD curves according to the equations below:
![]() | (1) |
![]() | (2) |
![]() | (3) |
![]() | (4) |
The morphology evolution of the PAN, CNF, and CNF-Ni samples at each fabrication step was also investigated by scanning electron microscopy (SEM, Fig. S2†). The fibers of the PAN film exhibit a slight shaggy surface with a diameter in the range of 175–300 nm and the averaged diameter is 219 nm. After the subsequent peroxidation and carbonization processes, a CNF film with smooth fiber surfaces was obtained. The CNF fiber diameter is in the range of 150–275 nm and the averaged diameter is 216 nm. The specific surface area (SSA) of the CNF film is 99.94 m2 g−1 (Fig. S3a†). There are two kinds of pores in the CNF film. The large ones are at the micrometer level, while the small micro- and mesopores are in the range from 1 to 10 nm with an average pore size of 4.44 nm, as shown in the Barrett–Joyner–Halenda (BJH) pore size distribution plot (Fig. S3b†). After the carbonization, the highly crosslinked CNFs form a 3D conductive network, which can reduce the contact resistance and facilitate the charge transport within the electrode (Fig. S4†).25 After the electrodeposition process, the CNFs were densely covered with a nickel layer with notable roughness and the diameter of CNF-Ni increased to 300–550 nm with an averaged diameter around 443 nm. The SSA of the CNF-Ni film is 8.51 m2 g−1 and the micro- and mesopore size distribution is in the range of 1–10 nm with an average pore size of 7.88 nm (Fig. S5†). The crystalline structure of the films was also confirmed by X-ray diffraction (XRD) characterization (Fig. S6†). After electro-deposition, the characteristic peaks of (111), (200) and (220) of Ni appeared, which is in good agreement with the PDF card (JCPDS no. 04-0850).
The adoption of nickel metallization also improved the wettability of the CNF film. The contact angle of the CNF film was reduced from 79° to 25° after nickel metallization (Fig. S7†), which indicates the CNF-Ni film is more hydrophilic than the pristine CNF film. The hydrophilic nature further facilitated the growth and binding of the Fe2O3 nanosheets.
![]() | ||
| Fig. 1 Schematic image showing the fabrication process of Fe2O3 nanosheets on the CNF-Ni conductive skeleton. | ||
The crystal structure of the α-Fe2O3 nanosheets was then examined by transmission electron microscopy (TEM) and X-ray photoelectron spectroscopy (XPS). The high-resolution TEM images (Fig. 3a and S9†) confirmed that the synthesized α-Fe2O3 sample contains a crystalline in amorphous heterogeneous structure. The red-dashed lines labeled the lattice fringes observed inside the α-Fe2O3 nanosheets, indicating crystalline parts of the sample surrounded by the amorphous counterpart. The amorphous Fe2O3 shall benefit the isotropic ion diffusion and thus improve the cycling performance of the anode. The inset selected area electron diffraction (SEAD) pattern is also consistent with the (104) and (116) planes of α-Fe2O3. The XPS full-spectrum (Fig. S10†) confirms the existence of Fe and O elements. High-resolution Fe 2p spectrum (Fig. 3b) shows two characteristic peaks located at 710.8 and 724.6 eV corresponding to Fe 2p1/2 and Fe 2p3/2 spin orbitals of Fe2O3, together with two satellite peaks at 717.0 and 733.0 eV.25,26 The fitting curves indicated a mixed-valence state of Fe2+ and Fe3+ inside the Fe2O3 nanosheets. The mixed-valence of iron cations will promote the formation of ionic and electronic defects, which shall benefit the redox reaction activities and thus the electrochemical performance of the anode.27 The high-resolution spectrum of O1s (Fig. 3c) can be fitted into two oxygen contributions. The peak at 531.9 eV corresponds to O2− in Fe2O3. The peak at 530.1 eV is attributed to defects and contaminants, suggesting the existence of surface species including hydroxyls, chemisorbed oxygen, and water molecules.
For comparison, the Fe2O3 nanosheets grafted on CNF (without surface metallization) with the same mass loading (namely, CNF@Fe2O3) was tested. SEM image of the CNF@Fe2O3 sample (Fig. S11a†) shows that the CNF is fully covered with the flocculent structure of Fe2O3. The high-magnification SEM image (Fig. S11b†) shows that Fe2O3 is not evenly grown on the surface of the CNF. Fig. S11c† illustrates the CV performance of the CNF@Fe2O3 with various scan rates ranging from 1 mV s−1 to 100 mV s−1. The CV curves are relatively rectangular at a low scan rate below 10 mV s−1. Beyond 10 mV s−1, the shape of the curve changed dramatically, indicating a decreasing charge/discharge capability. The GCD curves of the CNF@Fe2O3 electrode at various current densities of 2, 5, 10, 15 and 20 A g−1 show a higher IR drop than those of CNF-Ni@Fe2O3 (Fig. S11d†). This can be attributed to the ineffective infiltration of electrolyte and poor electronic transport in the CNF@Fe2O3 electrode.
Fig. 4c shows that the CNF-Ni@Fe2O3 electrode holds better rate performance than the CNF@Fe2O3 electrode. Electrochemical impedance spectroscopy (EIS) results show a clearly reduced electronic resistance of the anode after introducing the Ni layer (Fig. 4d). This indicates the surface-metallization facilitated the diffusion of ions and transportation of electrons, which would be beneficial for the long-term stability of the electrode. The CNF-Ni@Fe2O3 electrode exhibited superior capacitance retention of 85.1% after 100
000 cycles at a scan rate of 50 mV s−1 (Fig. 4e). After cycling, the Fe2O3 nanosheets still maintained its original morphology (Fig. S12†), indicating ultra-high stability of the sample with the CNF-Ni 3D conductive network. Table 1 compares the electrochemical performance of our CNF-Ni@Fe2O3 anode with other reported Fe2O3-based materials, which demonstrates remarkably improved specific capacitance and cycling stability of this earth-abundant Fe2O3 material.11,12,14,18,25,28–31
| Electrode | Electrolyte | Potential window | Capacitance | Cycling performance | Ref. |
|---|---|---|---|---|---|
| Fe2O3 | 0.5 M Na2SO4 | −0.8 to 0 V | 428.6 F g−1 (1.80 F cm−2) at 1 mV s−1 | 85.1% after 100 000 cycles |
This work |
94.4% after 50 000 cycles |
|||||
| Fe2O3 | 0.5 M Na2SO4 | −0.8 to 0 V | 418.7 F g−1 at 10 mV s−1 | 93.3% after 5000 cycles | 25 |
| Fe2O3–P | 1 M Na2SO4 | −0.8 to 0 V | 369 F g−1 at 1 mA cm−2 | 83% after 5000 cycles | 11 |
| Fe2O3 | 2.5 M Li2SO4 | −1 to 0 V | 701.4 F g−1 at 10 mV s−1 | 86.1% after 6000 cycles | 29 |
| Fe2O3 | 1 M Na2SO4 | −1 to 0 V | 228.8 F g−1 at 10 mV s−1 | — | 30 |
| Fe2O3@PPy | LiCl | −0.8 to 0 V | 207 mF cm−2 at 1 mA cm−2 | 97.2% after 5000 cycles | 28 |
| Ti–Fe2O3@PEDOT | 5 M LiCl | −0.8 to 0 V | 311.6 F g−1 at 1 mA cm−2 | 96% after 30 000 cycles |
14 |
| Fe2O3 | 5 M LiCl | −0.8 to 0 V | 89 F g−1 at 0.5 mA cm−2 | 95.2% after 10 000 cycles |
12 |
| Fe3O4@Fe2O3 | 1 M Na2SO4 | −0.8 to 0 V | 1.20 F cm−3 (231.9 F g−1) at 5 mV s−1 | 94% after 5000 cycles | 31 |
| Fe2O3/graphene | 1 M Na2SO4 | −1 to 0.3 V | 343.7 F g−1 at 3 A g−1 | 95.8% after 50 000 cycles |
18 |
The electrochemical performance of the CNF-Ni@MnO2 cathode was further investigated. CV curves under different scan rates ranging from 1 to 100 mV s−1 (Fig. 5b) show a typical rectangle-like shape due to the essential reversible successive redox reactions of the MnO2 active material.35,36 Despite a high mass loading of 5.1 mg cm−2, the CNF-Ni@MnO2 cathode still shows a high Cm value of 478.4 F g−1 at the scan rate of 1 mV s−1. The GD characteristics are investigated in the range of 1 to 20 mA cm−2 (Fig. S16†). No voltage plateaus were observed in the curves, which is consistent with the CV results. All the curves show standard isosceles triangle shapes, owing to the excellent ion and electron-transporting property.
In this study, two control samples were tested for comparison, including MnO2 nanosheets electrodeposited on nickel foam (NF) and CNF, with the same areal mass loading. Cracks can be clearly observed on the surface of the NF@MnO2 sample (Fig. S17†). Moreover, inhomogeneous and discontinuous structures composed of bulk and large particle appear around the CNF without the assistance of the Ni layer (Fig. S18†). It is likely that the inferior conductivity and weak surface wettability of CNF lead to uneven deposition of the MnO2 layer.
The areal capacitance of the CNF-Ni@MnO2 cathode reaches 2.44 F cm−2 at a scan rate of 1 mV s−1 and capacitance retention of 39.5% is observed even when the scan rate increases by 20-fold (Fig. 5c). Fig. S19a–d† shows the CV and GCD curves of CNF@MnO2 and NF@MnO2 electrodes. Lower Ca values of NF@MnO2 (1.97 F cm−2) and CNF@MnO2 (2.37 F cm−2) were observed at the same scan rate of 1 mV s−1. When the scan rate increases from 1 mV s−1 to 50 mV s−1, the capacitance retention of the CNF-Ni@MnO2 (22.6%) still outperformed the NF@MnO2 (18.6%) and CNF@MnO2 (7.7%) electrodes. CV curves of the three samples at the scan rate of 20 mV s−1 are shown in Fig. S19e† for better comparison. The CNF-Ni@MnO2 electrode also shows the best capacitance retention versus scan rates compared with the NF@MnO2 and CNF@MnO2 electrodes with the same mass loading (Fig. S19f†). The introduction of the Nickel layer also greatly reduced the impedance of the MnO2 electrode (Fig. 5d). Overall, the CNF-Ni@MnO2 cathode exhibits excellent capacitance retention of 108.2% after 26
000 cycles at a scan rate of 50 mV s−1 (Fig. 5e). The increase in specific capacitance may be related to defects formation and morphology change during MnO2 dissolution-redeposition upon cycling.37,38 These results further demonstrate that the surface metallization of CNF plays an important role in improving the pseudocapacitive properties of active materials.
The electrochemical stability of the pseudocapacitor device is evaluated through a CV cycling test at a scan rate of 50 mV s−1 for 11
000 cycles (Fig. 6e). The pseudocapacitor exhibits excellent cycling stability with 82.3% capacitance retention after successive 11
000 cycles. Importantly, to evaluate the energy and power densities of the pseudocapacitor, the data calculated from the GCD curves were compared with those of previously reported supercapacitor devices, such as Ni/MnO2-FP//Ni/AC-FP,39 Fe2O3/CFs//MnO2/CNT,40 CF/MnO2//Fe2O3/CF,11 MnO2//Fe2O3/PPy,28 typical Li-ion battery (4 V, 500 μA h)41 and commercial supercapacitor (5.5 V, 100 mF),42 as presented in the Ragone plot (Fig. S21†). Our pseudocapacitor exhibited a maximum energy density (Ev) value of 4.32 mW h cm−3 at the power density (Pv) of 10.29 mW cm−3 and maintains an Ev of 0.38 mW h cm−3 at the tested maximum Pv of 514.80 mW cm−3. Table S1† compared the recently-reported energy storage devices in detail, including areal capacitance (Ca), volumetric capacitance (Cv), maximum energy density (Emax) and maximum power density (Pmax). The Ca, Cv and Ev of our ASC device outperformed these devices. A soft pack pseudocapacitor was further fabricated in the lab (Fig. 6e). Such a device can drive 12 commercial LEDs in parallel connection simultaneously after shortly charging for 10 s.
000 cycles) and an ultra-high areal capacitance (428.6 F g−1 at a high mass loading of 4.2 mg cm−2), which outperformed state-of-art Fe2O3-based anodes. The excellent electrochemical performance of the Fe2O3-based anode was attributed to the introduction of the nickel metallization layer as well as the unique structure of the Fe2O3 anode. The nickel layer improved the electronic conductivity and wettability of the CNF substrate and enhanced the interface stability of the CNF-Ni@Fe2O3 composite. The crystal/amorphous interfaces of the Fe2O3 anode offer isotropic ion/electron diffusion pathways with high stress-tolerance upon long-term cycling. Such a high-performance pseudocapacitive anode shows promising opportunities in future energy storage applications. Adopting the interface nickel metallization method in a MnO2 cathode, excellent capacitance retention of 108.2% was reached after 26
000 cycles. We anticipate such an interface-management method can find a wider application in elevating the stability of metal oxide materials during redox reactions in various energy storage devices.
Footnotes |
| † Electronic supplementary information (ESI) available. See DOI: 10.1039/c9ra10285j |
| ‡ These authors contributed equally to this work. |
| This journal is © The Royal Society of Chemistry 2020 |