Open Access Article
Fujia Chena,
Yujiu Zhoua,
Jimin Guoa,
Song Suna,
Yuetao Zhao*b,
Yajie Yanga and
Jianhua Xu
*a
aState Key Laboratory of Electronic Thin Films and Integrated Devices, School of Optoelectronic Science and Engineering, University of Electronic Science and Technology of China, Chengdu 610054, China. E-mail: jianhuaxu215@163.com; Fax: +86-28-83206123; Tel: +86-28-83207027
bSchool of Electronics and Information, Jiangsu University of Science and Technology, Zhenjiang 212003, China. E-mail: zhaoyuetao@yeah.net
First published on 13th January 2020
High performance dielectric polymer materials are a key point for energy storage capacitors, especially film capacitors. In this paper, a sandwich-structured polymer film is constructed to achieve high energy density and high efficiency. High dielectric materials of poly(vinylidene fluoride-hexafluoropropylene) (P(VDF-HFP)) doped with barium titanate (BaTiO3) are used as the outer layer to achieve a high dielectric constant, and a boron nitride nanosheet (BNNS) layer is inserted between P(VDF-HFP)/BaTiO3 to obtain a high breakdown field strength of composite films. The results indicate that when the doping amount of the BaTiO3 nanoparticles reaches 10 wt% and the mass fraction of the BNNS layer is 0.75 wt%, a significant improvement of energy storage performance is obtained. The energy storage density of the P(VDF-HFP)/BaTiO3/BNNSs composite film can reach 8.37 J cm−3, which is higher than 6.65 J cm−3 of the pure P(VDF-HFP) film. Compared with the P(VDF-HFP) film doped with BaTiO3, significant improvement of the breakdown field strength (about 148.5%) is achieved and the energy storage density increases 235% accordingly, resulting from the inserted BNNSs layer blocking the growth of electrical branches and suppressing leakage current. This novel sandwich-structured film shows promising future applications for high performance dielectric capacitors.
(ε0 is the vacuum dielectric constant, and
is the relative dielectric constant of the material). Therefore, it is believed that the dielectric constant and breakdown field strength of the lifted material can effectively increase the energy storage density.
In general, compared with polymer materials, inorganic ceramic materials exhibit higher dielectric constant. In recent years, composite materials composed of polymer materials and inorganic ceramics have been widely studied.7–10 In order to increase the dielectric constant of polymer materials, the introduction of inorganic ceramic particles, such as BaTiO3 (BT), BaxSr1−xTiO3 (BST), P(Mg1/3Nb2/3)O3–PbTiO3, etc.,11–14 into polymer matrix is considered an effective method. However, in order to achieve a higher dielectric constant of the composite material, it is generally necessary to add a higher volume fraction of the ceramic materials, which leads to problems with the compatibility and dispersion of ceramic particles with the matrix. Hence, several kinds of research have been carried out to solve this problem: surface modification of ceramic fillers,15–17 regulation of filler distribution,18,19 the addition of third phase fillers, etc.20–22 Ceramic materials after surface treatment and structural control have better compatibility and dispersion.
Boron nitride nanosheets (BNNSs) are a typical two-dimension nanomaterial that have become an ideal filler for high performance polymer composites. It has a high forbidden bandwidth (≈6 eV) and a high intrinsic breakdown voltage.23,24 It is widely used in research to improve the energy storage characteristics of polymer materials. For example, BNNSs are directly added to the matrix, which resulted in a significantly improved breakdown field strength.21,25,26 Most of these work is centered around the direct compounding of fillers and polymer materials, as well as the uniform distribution of fillers in polymer composite films. However, the structural design of film is rarely studied. Recently, Huang et al. used the structural design of BNNSs insulation layer to improve the breakdown field strength and reduce the loss.27 This structure has been proven very reliable for increasing energy storage density. In order to improve the energy storage characteristics of materials, BaTiO3 nanoparticles were chosen as the ceramic filler to increase the dielectric constant of the matrix. At the same time, considering that BaTiO3 will cause a decrease in breakdown field strength, inspired by their work,27 BNNSs were chosen as the third phase filler and designed as a separate mezzanine. While using the inorganic ceramic particles to increase the dielectric constant, the effect of suppressing the reduction of breakdown field strength is achieved by adding BNNSs. Through the coordination between the materials of each phase, it should be an effective way to increase the dielectric constant while suppressing a significant reduction in breakdown strength. As for details, P(VDF-HFP) is selected and a sandwich structure polymer films are constructed. High dielectric materials of P(VDF-HFP) doped with BaTiO3 are used as the outer layer, and a BNNSs layer is inserted between P(VDF-HFP)/BaTiO3. Different from the method of directly doping BNNSs into the matrix material, the separate mezzanine is prepared by solution casting. Each layer structure is sequentially prepared on the quartz substrate by a scraper from bottom to top, finally forming a sandwich composite film. In addition, BaTiO3 nanoparticles are surface-modified with dopamine to improve the dispersion of nanoparticles in the matrix. The sandwich-structured film presents a significant improvement in dielectric constant and energy storage density, the breakdown field strength of the composite film is not seriously reduced by the addition of BaTiO3. For instance, the sandwich-structured film has a dielectric constant of 10.99, which is 1.446 times of pure P(VDF-HFP), and the energy storage density has also improved significantly. This work provides a new way to obtain high performance energy storage media composites.
First of all, ultrasonic degradation method which is reported previously is applied here to prepare BNNSs.21,26,28 2 g h-BN was added to 200 mL DMF solvent, continuously stripping by ultrasonic breaker for 20 h (340 W). After the completion of the ultrasonic, the solution was placed in a centrifuge and centrifuged at 3000 rpm for 45 min, then the supernatant was collected and centrifuged again at 9000 rpm for 10 min. In order to ensure the dispersion of BNNSs, freeze-drying method was used to dry the precipitate at the bottom of the centrifuge tube. As reported in the literature, BNNSs were prepared by ultrasonic degradation method with a yield of 2.5–3%.27,29 The experimentally collected BNNSs were 60 mg, and the acquisition rate was within the normal range. The experimental results preliminary indicated that h-BN was stripped successfully.
In addition, barium titanate nanoparticles was coated by dopamine through water bath.30 0.04 g of dopamine hydrochloride was dissolved in an aqueous ammonia solution with pH of 8.5 to form a mixed solution of 2 g L−1. Appropriate amount of BaTiO3 nanoparticles was added to the above solution, and stirred in a water bath at 60 °C for 12 h. The product was collected by centrifugation. Finally, BT@DPA particles were vacuum dried at 60 °C for 10 h.
The specific experimental process can be seen in Fig. 1. Pure P(VDF-HFP) was first physically blended with 10 wt% of BT@DPA nanoparticles in DMF solvent and mechanically stirred for 12 h until P(VDF-HFP) was completely dissolved. The BNNSs were dispersed in isopropanol to form a solution with 0.75 wt%. The preparation process of the sandwich-structured film was as follows. Firstly, a P(VDF-HFP)/BT@DPA bottom layer film was casted on a quartz substrate with a scraper, dried at 70 °C for 6 hours in a vacuum oven to remove solvents. Then, the interlayer of BNNSs and the top layer film were casted through the same process. The sandwich-structured film was dried overnight in a vacuum oven at 70 °C to remove the solvents. Finally, the quartz substrate was placed on a heating table at 200 °C for 10 min and quenched in ice water. Hereinafter, this sandwich-structured film is named PBP/BT@DPA. In addition, a solution of only doped with BaTiO3 nanoparticles and a solution of co-doped with BaTiO3 nanoparticles and BNNSs (the doping amount of BNNSs and BaTiO3 were 10 wt%) were prepared. The same preparation process was used to prepare four other films: pure P(VDF-HFP), P(VDF-HFP)/BT, P(VDF-HFP)/BT@DPA, HFP/BT@DPA/BNNSs, all of which were single layer (the thickness were 12–13 μm).
![]() | ||
| Fig. 1 Experimental flow chart: surface modification of BaTiO3 by dopamine, preparation of BNNSs and fabrication of sandwich structure film. | ||
A series of morphological characterization and electrical performance tests on the prepared materials and films were performed. First of all, BNNSs were characterized by Atomic Force Microscope (AFM) and Transmission Electron Microscope (TEM) respectively. The cross section of the films were observed by Scanning Electron Microscopy (SEM, Hitachi S-4800). In addition, the films were characterized by Fourier-transform infrared spectroscopy (FTIR, 8400S, Shimadzu) and X-ray diffraction (XRD, Malvern Panalytical, Inc.). The thickness of film was measured by a magnetic induction thickness-meter (Fischer DUALSCOPE MPO). Finally, dielectric spectrum characteristics were measured by using a precision impedance analyzer (4294A, Agilent Technologies, Inc.) from 40 Hz to 5 MHz. Breakdown field strength was tested with a withstand voltage tester (TH9120, Changzhou Tonghui electronics co., LTD), and P–E hysteresis loops of films were measured by using a ferroelectric tester (Radiant Technologies, Inc.).
![]() | ||
| Fig. 2 Micromorphology of BNNSs: (a) AFM image, (b) TEM characterization images and (c) the thickness of a piece of BNNSs intercepted. | ||
![]() | ||
| Fig. 3 SEM images of film cross section: (a) P(VDF-HFP)/BT, (b) P(VDF-HFP)/BT@DPA, (c) HFP/BT@DPA/BNNSs and (d) PBP/BT@DPA. | ||
FTIR and XRD results are visible in the ESI.† FTIR technology is a productive method to identify the different crystal phases of PVDF-based polymers, and the spectra of films are demonstrated in Fig. S1.† P(VDF-HFP) is a polar polymer with a long molecular chain extending from the crystalline region to the amorphous region. The absorption peaks at 879 cm−1 are the amorphous phase absorption peak of P(VDF-HFP), while the absorption peaks at 764 cm−1 and 796 cm−1 are the α phase absorption peaks of P(VDF-HFP) film.31,32 These films mainly exhibited α phase, indicating that the preparation process used had no significant effect on the crystalline phase of the matrix material. Analyzing the XRD results in Fig. S2,† the characteristic diffraction peaks of BaTiO3 are very obvious, and the diffraction peaks of BaTiO3 at (100), (110), (111) crystal planes can be clearly seen.33,34 It is worth noting that a diffraction peak appears at 2θ ≈ 26.4°, corresponding to the BNNSs (002) crystal plane.21,35 Because the amount of BNNSs added to the composite film is small, the peak intensity is very weak due to the influence of the BaTiO3 diffraction peak.
decreases with increasing frequency, due to the periodic transformation of the electric field at high frequency resulting in the decrease of charge distribution in the direction of the electric field. In other words, the role of the molecular dipole moment is gradually reduced. It can be seen from the figure that the dielectric constant of the composite film doped with BaTiO3 is much higher than that of the pure P(VDF-HFP) film. The
of PBP/BT@DPA at 1 kHz is 10.99, while the pure P(VDF-HFP) film is only 7.6, which shows a very large enhancement rate of
(144.6%). In contrast, the
of HFP/BT@DPA/BNNSs is not increase significantly, because the doping amount of BNNSs is 10 wt% and its dielectric constant is inherently low (∼4). The result shows that the effect of BaTiO3 on the improvement of dielectric constant is very obvious. The dielectric loss tan
δ of all films shows a gradually rising trend.36 Compared with pure P(VDF-HFP) film, the composite film doped with BaTiO3 particles shows a higher loss at low frequency. On the one hand, Maxwell–Wagner–Sillars (MWS) polarization dominates the dielectric response at low frequencies. On the other hand, the addition of BaTiO3 particles also increases the dielectric loss.37,38 The loss increases rapidly at high frequencies, which can be attributed to the dynamic relaxation of the matrix material.39 The dielectric loss of HFP/BT@DPA/BNNSs film is much larger than other films, this data validates the results of the SEM. The dielectric loss of the polymer is not only related to the nature of the material itself, but also to the state of aggregation between the phases.40,41 The agglomeration and local accumulation of ceramic particles directly increase the porosity of the mixture and increase the water absorption of the composite. When there are many pores in the matrix, the phase composition of each material in the actual matrix deviates from the theoretical value, and the dielectric loss increases by order of magnitude. The moisture absorption of pores will increase the moisture content of the dielectric material, which has a great influence on the dielectric loss. The insulation layer of BNNSs are separately added into sandwich-structured film, avoiding mutual aggregation between the phases, which reduces the porosity of the composite and achieves better interface conditions. Compared with the film directly doped with two kinds of inorganic materials, this structure makes the density distribution of the film more uniform, which is very helpful for improving the dispersion of the filler. However, the insulation layer of BNNSs doesn't significantly reduce the dielectric loss at high frequency. This may be due to the large amount of BaTiO3 added, and the effect of suppressing the loss of BNNSs is not conspicuous. Ceramic fillers can effectively increase the dielectric constant, but the content is often high, which also weakens the flexibility of the polymer film. Compared with PVDF, P(VDF-HFP) has a lower glass transition temperature and a higher degree of amorphization, resulting in abetter flexibility. This is the reason why P(VDF-HFP) is chosen as the matrix material.42,43 In short, the composite film with BNNSs interlayer shows a great improvement in dielectric properties. Not only does the dielectric constant increases significantly, but also the dielectric loss is suppressed to some extent.
![]() | ||
Fig. 4 Dielectric spectrogram: relationship between dielectric constant and dielectric loss (tan δ) as a function of frequency. | ||
| P(E) = 1 − exp((−E/Eb)β), |
| Materials | (1 kHz) | Eb (kV mm−1) | Ue (J cm−3) | References |
|---|---|---|---|---|
| PBP/BT@DPA | 10.99 | 414.76 | 8.37 | This work |
| Polypropylene (PP) | 2.2 | 640 | 1–1.2 | 5 |
| Polyester (PET) | 3.3 | 570 | 1–1.5 | 5 |
| Polycarbonate (PC) | 2.8 | 528 | 0.5–1 | 5 |
| PVDF | 8 | 400 | 2.8 | 44 |
| PVDF/BST-NPs | 36 | 250 | 3.9 | 45 |
| 8 wt% BNNSs/PVDF | 8.3 | 486 | 7.25 | 46 |
| 0.5 wt% BaTiO3@BNNSs/PVDF | 12.5 | 350 | 7 | 47 |
| 7 vol% Fe3O4@BNNSs/PVDF | 16 | 300 | 7.1 | 21 |
| 7.5 vol% F–TiO2/P(VDF-HFP) | 12 | 160 | 1.4 | 48 |
| 5 vol% BaTiO3@PMPCS/P(VDF-HFP) | 20 | 300 | 7.5 | 49 |
| 0.4 wt% BNNSs/P(VDF-CTFE) | 23 | 300 | 6.8 | 50 |
P–E hysteresis loops and leakage currents of several films are visible in the ESI,† and the charge–discharge efficiency are shown in Fig. 6(a). The efficiency of the film doped with BaTiO3 decreases very sharply with the increase of electric field, and the charge–discharge efficiency is less than 50% at 200 kV mm−1. Compared with P(VDF-HFP), the efficiency of the sandwich-structured film does not decrease significantly. As the electric field strength increases, the difference in electrical properties between the base material and the filler causes an increase in the charge carrier concentration of the film, thereby causing a decrease in charge–discharge efficiency during the electric field switching process. BNNSs have a high length height ratio and specific surface area, and the high energy barrier of the nanosheets can suppress the movement of charges under high electric fields.51 The interlayer formed by solution casting has a dense network structure and plays a vital role in hindering the migration of charge carrier.52 In Fig. 6(b), the insulation resistivity of the film was calculated according to leakage currents. The leakage current of the dielectric film can be expressed as:
| IL = U/RI, |
| RI = ρId/A, |
Under low electric field, the conductive effect of BaTiO3 is not obvious, so the HFP/BT@DPA/BNNSs film with 10 wt% BNNSs added shows the highest insulation resistivity. As the electric field strength increases slowly, the conduction of BaTiO3 is also gradually enhanced. Meanwhile, the role of the BNNSs interlayer is gradually becoming prominent, which hinders the conduction of leakage current. Under the same electric field strength, sandwich structure film has a higher insulation resistivity.
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: 10.1039/c9ra09780e |
| This journal is © The Royal Society of Chemistry 2020 |