Bilayer graphene/HgCdTe based very long infrared photodetector with superior external quantum efficiency, responsivity, and detectivity

Shonak Bansala, Kuldeep Sharmaa, Prince Jaina, Neha Sardanab, Sanjeev Kumarc, Neena Guptaa and Arun K. Singh*a
aDepartment of Electronics and Communication Engineering, Punjab Engineering College (Deemed to be University), Sector-12, Chandigarh-160012, India. E-mail: arun@pec.ac.in
bDepartment of Metallurgical and Materials Engineering, Indian Institute of Technology, Ropar, India
cDepartment of Applied Sciences, Punjab Engineering College (Deemed to be University), Sector-12, Chandigarh-160012, India

Received 15th September 2018 , Accepted 13th November 2018

First published on 27th November 2018


Abstract

We present a high-performance bilayer graphene (BLG) and mercury cadmium telluride (Hg1−xCdx=0.1867Te) heterojunction based very long wavelength infrared (VLWIR) conductive photodetector. The unique absorption properties of graphene enable a long carrier lifetime of charge carriers contributing to the carrier-multiplication due to impact ionization and, hence, large photocurrent and high quantum efficiency. The proposed p+-BLG/n-Hg0.8133Cd0.1867Te photodetector is characterized and analyzed in terms of different electrical and optical characteristic parameters using computer simulations. The obtained results are further validated by developing an analytical model based on drift-diffusion, tunneling and Chu's methods. The photodetector has demonstrated a superior performance including improved dark current density (∼1.75 × 10−14 µA cm−2), photocurrent density (∼8.33 µA cm−2), internal quantum efficiency (QEint ∼ 99.49%), external quantum efficiency (QEext ∼ 89%), internal photocurrent responsivity (∼13.26 A W−1), external photocurrent responsivity (∼9.1 A W−1), noise equivalent power (∼8.3 × 10−18 W), total noise current (∼1.06 fA), signal to noise ratio (∼156.18 dB), 3 dB cut-off frequency (∼36.16 GHz), and response time of 9.4 ps at 77 K. Furthermore, the effects of different external biasing, light power intensity, and temperature are evaluated, suggesting a high QEext of 3337.70% with a bias of −0.5 V near room temperature.


Introduction

Infrared (IR) photodetectors have been successfully demonstrated from a wide variety of narrow bandgap semiconductors (Si and Ge)1–3 and alloys including III–V (InAs1−xSbx, InAs, GaAs),4–6 IV–VI (Pb1−xSnxTe),4 II–VI (Hg1−xCdxTe, CdZnTe, CdSeTe).4,7–10 These materials absorb the incident photon energy corresponding to their bandgaps and result in the output photocurrent.11 InSb, a III–V compound semiconductor material was first used for IR detection. The IR detection region is categorized into short wavelength IR (SWIR: 1–3 µm), mid wavelength IR (MWIR: 3–5 µm), long wavelength IR (LWIR: 8–14 µm) and very long wavelength IR (VLWIR: 14–30 µm) ranges.12 The potential applications of IR photodetectors include biomedical and thermal imaging, gas sensing, night vision, spectroscopy, and free space communication etc.4,13–15 Rapid advances are being made in developing inexpensive narrow bandgap semiconductor photodetectors with improved sensitivity and longer wavelengths. As a result, low dimensional structures, including quantum-well, quantum-dot, and quantum-wire, based IR photodetectors are reported with improved performances, but with expensive fabrication processes.16–19 On the other hand, the low leakage current, tunable bandgap, better stability, low thermal generation rate and relatively high absorption coefficient make the ternary alloy mercury cadmium telluride (MCT: Hg1−xCdxTe) a suitable material for high performance IR detectors.12,14,20–22 So far, numerous Hg1−xCdxTe-based IR photodetectors with different configurations such as p–n,23,24 p–i–n,14,25 dual band IR detector,15,26 and avalanche photodiode27 have been reported at cryogenic temperatures. The high dark current limited by Auger recombination processes and low temperature operations are the major disadvantage of MCT based IR photodetector.14,20,28,29 Hence, there is a requirement to design and develop MCT based IR photodetectors demonstrating higher efficiencies near room temperature.

The excellent electrical and optical properties of graphene (Gr) enables utilisation of Gr as a transparent electrode integrated with conventional photodetectors for ultraviolet (UV) to IR regions.30 The Gr/semiconductor heterojunction based photodetectors are expected to demonstrate a low dark current, low power dissipation, small parasitics, higher breakdown voltage, and high response speed than that of conventional homostructures. The Gr has been successfully composited with different materials like ZnO,31,32 Si,33 CdS34 (for UV applications), CdSe,35 GaN36 (for visible applications), and Si,1,37 Ge,3 PbS,38 GaAs39 (for IR applications). However, the zero bandgap and small optical absorption (∼2.3%) of monolayer graphene (MLG) result in limited photocurrent responsivity (<1 A W−1) and photocurrent (Ilight) to dark current (Idark) ratios (Ilight/Idark).6,30,33,40–42 Accordingly, several efforts including utilisation of few layer graphene, Gr quantum dots, inducing small bandgap in Gr layers using either doping or under transverse electric fields are made to improve the charge injection and separation, suppressing dark current with improved efficiency.11,13,43–46 The intentional doping in monolayer and bilayer Gr shifts the Fermi-level either upward or downward, creating a bandgap opening.47 To the best of our knowledge, a maximum bandgap of 430 meV is found in p-doped bilayer graphene (BLG).48 Xu et al.49 demonstrated 25 times higher electrical conductance and optical transmittance of 80% from few layer (5–10) graphene transferred onto MCT substrate in the MWIR spectral region at 77 and 300 K. Despite such studies, no photodetector combining BLG with MCT is successfully studied yet. Hence, here we propose and simulate a BLG/MCT based photodetector providing excellent light absorption and electron transport. The device exhibits a low dark current and high temperature operation due to lower thermo-generation rate. In this work, we investigate the effect of different external bias, incident light power intensity and temperature on the performance of proposed heterojunction photodetector. It is evident from the results that high external quantum efficiency (QEext) (>100%) is achieved due to long lifetime of photo-induced hot carriers in the VLWIR spectral region. The obtained results are further validated by developing an empirical model based on drift-diffusion, tunneling and Chu's methods in VLWIR, suggesting potential applications in next-generation high-performance, ultra-low-power, and cost-effective IR photodetectors for optoelectronics devices.

Device structure and description

The inset of Fig. 1a shows the schematic of proposed BLG composite Hg1−xCdx=0.1867Te based VLWIR photodetector. The highly doped p+-type BLG conformably cover 10.0 µm wide lightly doped n-type Hg0.8133Cd0.1867Te to form a heterojunction photodetector. The p+-doping of the Gr is typically being achieved through the chemical doping with HNO3,50,51 FeCl3,52 AuCl3,53,54 SOCl2,55,56 and NbCl5 (ref. 57) utilising chemical vapor deposition (CVD) technique. Practically, the Gr layers can be directly mechanically exfoliated or be transferred to suitable substrate utilizing Cu films in CVD growth techniques without any contamination issues.58 The electrical ohmic contacts of aluminium (Al) are made as anode and cathode to collect the photo-generated charge carriers. The nominal thickness of 2 nm for BLG is considered for our studies which is in consonance with previously reported values.59–61 The proposed p+-BLG/n-Hg0.8133Cd0.1867Te photodetector can be grown on lattice matched CdZnTe substrate. CdZnTe substrate is chosen because MCT/CdZnTe interface offers less interface trap charge as compared to Si, Ge, and CdTe substrates.24 In this paper, we have not considered the substrate effect, as it does not affect the device performance significantly. The Silvaco Atlas software is utilised to design and evaluate the electrical and optical performances of BLG/HgCdTe photodetector. The VLWIR radiations are incident from the p+-BLG cladding window over the narrow bandgap n-Hg0.8133Cd0.1867Te active/absorbing layer. The p+-BLG is used as a light absorber. The lightly doped n-Hg0.8133Cd0.1867Te generates total dark current and photocurrent. The bandgap and doping concentration of active region are selected to give better absorption of VLWIR radiations suppressing thermally generated carriers. In order to simulate the device, a bandgap of 250 meV for BLG is considered.62,63 When VLWIR light illuminates the p+-BLG/n-Hg0.8133Cd0.1867Te heterojunction, the hot photo-carriers transport from the active layer to the Gr layer due to built-in electric field (Ebuilt-in).64 As a result, the change in graphene conduction is observed according to the relation, Δσ = Δnqµ,65,66 where Δn represents variation in carrier-concentration of graphene; q corresponds to the electronic charge; and µ is the carrier mobility. The schematic illustration of depletion region with a barrier height (ϕB) between the BLG and HgCdTe is given in Fig. 1b. The presence of potential barrier within the heterojunction is due to the existence of gradients in electron affinity ∇χ and electrostatic potential ∇V. The electrons are dominated charge carriers than holes. The electrons travel from n-region into the lower energy states in p+-region, leaving the positively charged empty states in the n-region. Accordingly, the energy band bends upward in the vicinity of the p+–n heterojunction to form an Ebuilt-in. The doping profile of the material determines the barrier height, however, potential variation results in energy band drop at p+–n interface junction23 as shown in Fig. 1a and b. The existence of the small bandgap in Gr due to doping will change the work function of Gr resulting in shifting of Fermi-level towards the conduction band. This makes graphene different than the others 2D semiconductor materials.67 It is also observed from Fig. 1b that under illumination, the photo-induced carriers accumulate in the potential well, raising the Fermi-level and increasing the conductivity of the device. The energy band diagram of the device can be explained by the classical theory of Anderson.68 The absorbed photo carriers undergo hot carrier multiplication (CM) by impact ionization (also known as inverse Auger recombination process)69–72 in p+-BLG, subsequently cross the barrier through internal photoemission (IPE) process (in picosecond scale),33 and finally be collected by n-Hg0.8133Cd0.1867Te contributing the total photocurrent. The carrier multiplication factor can further be tuned with chemical doping.73,74 The fast recombination rate (in picosecond) of the photogenerated carriers results in a maximum multiplication factor of 4.3 by the impact ionization process.75 Thus carrier multiplication, i.e. internal gain mechanism in BLG will enhance the photocurrent Ilight of the device due to the increase in carriers.76 The increase in photocurrent will result in higher internal quantum efficiency (QEint),33 facilitates to break through the upper-limit of traditional MCT based IR photodetectors. This indicate that our BLG composite photodetectors can still work effectively under a low illumination conditions. In our device, we have achieved a carrier multiplication factor of 1.25 for p+-doped graphene at 250 K, which is in good agreement to the earlier reported values.73,74 In addition, an equivalent Mixed-Mode circuit is utilised for estimating device performances in dark condition as shown in Fig. 1c. It consists of an equivalent diode in parallel with shunt resistance Rsh, junction capacitance Cj, and load resistance RL with series resistance Rs at an applied bias V for generating carriers contributing to the device current. The effect of illumination is implemented by a constant current source Ilight in Silvaco Mixed-Mode simulator.
image file: c8ra07683a-f1.tif
Fig. 1 (a) The simulated energy bandgap diagram of p+-BLG/n-Hg0.8133Cd0.1867Te VLWIR photodetector at zero-bias (V = 0 V) under no illumination conditions. Here, ECB and EVB represent conduction and valence band energies, respectively; EF is Fermi-level energy; Egp and Egn are the bandgap of p+- and n-regions, respectively; Vip and Vin are the potential barriers in p+- and n-regions, respectively. The schematic of proposed photodetector is shown in the inset. The VLWIR radiations with an illumination cut-off wavelength of 20.6 µm are incident on the p+-BLG. Here, tp+ and d are the thickness of p+- and n-regions, respectively. V and RL represent the applied bias and load resistance, respectively. (b) The schematic energy bandgap diagram of proposed photodetector under illumination and reverse bias condition. Here, E0 is the vacuum energy level; EFp and EFn are Fermi-level energies of p+- and n-regions, respectively; ϕB is the barrier height and χn is the electron affinity of the n-region. ϕp and ϕn denote the work function of p+- and n-regions, respectively. Under illumination the photo-induced carriers accumulate in the potential well, raising the Fermi-level and increasing the conductivity of the device. (c) The equivalent circuit of proposed BLG/MCT photodetector indicating photocurrent (Ilight), junction capacitance (Cj), shunt resistance (Rsh) and series resistance (Rs) is utilised for evaluating dark current properties in Silvaco Mixed-Mode circuit simulations.

In self-powered mode, the depletion layer width w = [2ε0εr1εr2(VbiV)(NA2 + ND2)/(q(εr1NA + εr2ND)NAND)]1/2 of the heterojunction is found to be 64.28 nm for a built-in potential (Vbi = Vip + Vin) of 21 mV. Here, Vip and Vin are the barriers corresponding to energy band bending at p+- and n-regions, respectively. ε0 is the absolute permittivity and εr1 & εr2 represent the relative permittivity in p+- and n-regions, respectively. NA (2 × 1022 cm−3) and ND (1 × 1016 cm−3) corresponds to the acceptor and donor doping concentrations in p+- and n-regions, respectively. The thickness of bilayer graphene is considered to be 2.0 nm, which is considerably smaller than that of MCT (10.0 µm). Accordingly, the depletion region extends inside the MCT (n-side) resulting in gradual shrinkage in band diagram towards BLG/MCT interface as observed in Fig. 1a employing computer simulations. The junction capacitance Cj = ε0εr2A/w in self-powered mode is found to be 0.98 fF. The device exhibits the transit time τtr = w/vsatn of 6.4 ps, where vsatn is the carrier saturation velocity (106 cm s−1) in n-region. The dependence of εr2 on x composition for n-region is approximated by:12

 
εr2(x) = 20.5 − 15.6x + 5.7x2 (1)

Results and discussions

Electrical characterization

The p+-BLG/n-Hg0.8133Cd0.1867Te photodetector is electrically characterized by solving continuity, carrier transport and Poisson equations with optimized boundary conditions as approximated by Boltzmann's transport model.15 Here, BLG is considered as 3D in nature analogous to earlier reported studies demonstrating the integration of multilayer graphene with other conventional semiconductors which couples 2D transport equations to 3D equations.67 A 2D semiconductor material has one physical dimension of the order of Fermi wavelength λF. In our case, image file: c8ra07683a-t1.tif of graphene is estimated to be around 0.56 nm for the sheet carrier density (n) of 4 × 1015 cm−2. The obtained value of λF is smaller than the considered thickness of doped BLG (2 nm), hence, it is necessary to consider 3D equations for estimating device characteristics. Further, to reproduce the carrier transport in graphene a drift-diffusion approach is implemented to degenerate semiconductor and parabolic shape of the conduction band.77 The Newton–Richardson iteration method and concentration dependent Analytic model are used to estimate the carrier mobility in the photodetector.15,24 In order to characterize the carrier lifetime and the dark current in the proposed photodetector, Shockley–Read–Hall (SRH), Auger, optical (band-to-band), trap assisted tunneling (TAT), and band-to-band (BTB) standard tunneling mechanism models are considered. The doping and carrier densities are evaluated using Fermi–Dirac statistics.15,24,78

The performance of the photodetector at 77 K is evaluated analytically for the operation at the wavelength of 20.6 µm. The photons having energy greater than the bandgap create electron–hole pairs in the lightly doped n-region. The mole fraction x of cadmium in the Hg1−xCdxTe tunes the energy bandgap in VLWIR with a cut-off wavelength of 20.6 µm. For n-Hg1−xCdxTe, the energy bandgap (Egn), electron affinity (χn), and intrinsic carrier concentration (nin) as a function of x composition and lattice temperature T are approximated by eqn (2), (3) and (4), respectively.12,24,79

 
image file: c8ra07683a-t2.tif(2)
 
χn(x,T) = 4.23 − 0.813 × [Eg(x,T) − 0.083] (3)
 
image file: c8ra07683a-t3.tif(4)
where, k is the Boltzmann constant.

The electron effective mass image file: c8ra07683a-t4.tif of n-Hg1−xCdxTe material is estimated by using Weiler's expression80 (eqn S1 and S2). The various computation parameters based on previous studies including effective density of states for electrons (NCB) and holes (NVB) in conduction and valence bands, respectively, intrinsic carrier concentration (ni), and carrier (electron and hole) lifetimes are listed in Table 1.12,24,67,81 Fig. 2 shows the triangular shape built-in electric field profile across p+–n heterojunction VLWIR photodetector for different biasing conditions. The maximum value of electric field (Emax) is found to be 17.8, 45.4, and 64.6 kV cm−1 at the heterojunction of the device with an external bias of 0, −0.5, and −1 V, respectively. The electric field E(x) across the device can be written as:

 
image file: c8ra07683a-t5.tif(5)
where xp+ and xn are the depletion width in p+- and n-regions, respectively.

Table 1 Optimised simulation parameters used for device analysis
Parameters p+-BLG n-Hg1–xCdxTe
x Composition 0.1867 (cal.)24
Bandgap (meV) (250)67,81 60.2 (cal.)24
Affinity (χ) (eV) (4.2)67,81 4.25 (cal.)24,79
Relative permittivity (εr) (3.3)67,81 17.8 (cal.)12,24
NCB (cm−3) (5.2 × 1016)67,81 1.0285 × 1015 (cal.)79
NVB (cm−3) (5.2 × 1016)67,81 1.3310 × 1018 (cal.)79
ni (cm−3) 3.4312 × 108 (cal.)79 3.8213 × 1014 (cal.)24
NA (cm−3) 2 × 1022 (assumed)
ND (cm−3) 1 × 1016 (assumed)



image file: c8ra07683a-f2.tif
Fig. 2 The electric field profile across the device at different external biasing conditions demonstrate high electric field at the p+–n heterojunction of BLG and MCT.

BLG is atomically thin with a thickness of the order of nm. This may create the depletion region width xp+ either almost fully depleted or very thin (≈3.21 × 10−16 m in our case), hence, can be safely neglected. The electron–hole pairs from MCT can be effectively separated by high built-in Ebuilt-in to generate the photocurrent. The dark current density (Jdark) is a combination of diffusion current density (JDIFF) in the neutral p+- and n-regions, drift current density (JGR) due to generation–recombination of charge carriers in the depletion region and the tunneling current density (JTUN). JTUN consists of the contribution of both the trap-assisted tunneling (TAT) and band-to-band (BTB) tunneling. Accordingly, the total dark current density as a function of voltage and ambient temperature is given by:

 
Jdark(V,T) = JDIFF + JGR + JTAT + JBTB (6)

The total diffusion current density is evaluated as:24

 
JDIFF = [(Jp)n + (Jn)p](e(qV/kT) − 1) (7)
where V represents the applied bias voltage, the diffusion component of current density for holes (Jp)n and electrons (Jn)p in n- and p+-regions, respectively, are given as:
 
image file: c8ra07683a-t6.tif(8)
 
image file: c8ra07683a-t7.tif(9)
where nin and nip are the intrinsic carrier concentrations in n- and p+-regions, respectively. µp and µn are the hole and electron mobilities, respectively. τp and τn represent the hole and electron lifetimes, respectively. γp = SpLp/Dp and γn = SnLn/Dn are the ratios of surface to bulk recombination velocities in p+- and n-regions, respectively. Here, Sp = 103 cm s−1 and Sn = 105 cm s−1 are the surface recombination velocities of holes and electrons, respectively at the heterojunction.24image file: c8ra07683a-t8.tif and image file: c8ra07683a-t9.tif are the diffusion lengths of holes and electrons. Dp = µpkT/q and Dn = µnkT/q represent the diffusion coefficients of holes and electrons, respectively. The valence and conduction band-edge discontinuities, after the formation of the p+–n heterojunction are given by ΔEVB (=ΔEg − ΔECB) and ΔECB (=χnχp). χn and χp are the electron affinities of the wide and narrow bandgap materials, where χn > χp. ΔEg (=EgpEgn) is total bandgap discontinuity and Egp and Egn represent the energy bandgaps in the p+- and n-regions.

The transfer of charge carriers across the p+–n heterojunction is strongly affected by the trap levels at the heterojunction particularly in depletion region. The electron and the hole components of current density due to the generation–recombination in the depletion region is given as:82

 
image file: c8ra07683a-t10.tif(10)
where τSRH = 1/σNfvth is SRH generation–recombination lifetime of carriers. σ = 6.9591 × 10−16 cm2 represents the capture cross section of minority carriers. Nf is the SRH trap density. image file: c8ra07683a-t11.tif is the thermal velocity of minority carriers.

The current related to TAT corresponds to the tunneling of electrons to the conduction band via a trap level within the bandgap. These trap states are the intermediate energy levels generated due to the existence of impurities in the material. The TAT component of current density is evaluated as:82

 
image file: c8ra07683a-t12.tif(11)
where
 
image file: c8ra07683a-t13.tif(12)
Here, Nt is the trap density different from SRH trap density, and h is the Planck's constant. Wc and P represent matrix elements associated with the potential and interband matrix elements, respectively. The position of the trap levels in the bandgap is indicated by Et.

The high reverse bias causes bending in energy band to tunnel the electrons from valence band to the conduction band as shown in Fig. 1. This BTB current density is given by:82

 
image file: c8ra07683a-t14.tif(13)
where = h/2π is the reduced Planck's constant, E represents the electric field across the depletion region.

Fig. 3a shows the simulated current density (J) as function of applied voltage varying from −1.0 to 0.3 V. The results are obtained under dark condition, and at a radiation of incident power intensity (Pin) of 1 W cm−2 at 20.6 µm. For the Mixed-Mode simulations of the circuit shown in Fig. 1c under dark condition, the values of Ilight, Cj, and Rsh are obtained at zero-bias condition. The proposed photodetector exhibits a low dark current density of 1.75 × 10−14 µA cm−2 and a photocurrent density of 8.33 µA cm−2 at zero-bias (self-powered mode) which in turn improves the signal-to-noise ratio (SNR), and hence specific detectivity. The simulated values of JdarkV characteristic are well in accordance with the values obtained from the analytical modeling. The obtained Jdark is smaller than that of the state-of-art photodetectors such as Hg1−xCdxTe based IR photodetector,24 Gr-Silicon Schottky IR photodetector,1 Gr-Germanium Schottky IR photodetector,3 Gr-GaAs IR photodetector39 and armchair graphene nanoribbons IR photodetector.83


image file: c8ra07683a-f3.tif
Fig. 3 The electrical characteristics of p+-BLG/n-Hg0.8133Cd0.1867Te heterojunction VLWIR photodetector at a cut-off wavelength (λc) of 20.6 µm. (a) The current density (J) and net resistance area product (RA)NET as a function of applied voltage (V) at 77 K under dark and illumination conditions with Pin = 1 W cm−2. Here, the values of Ilight, Cj, and Rsh are obtained at zero-bias condition and are used for Mixed-Mode simulation to evaluate device performances in the dark condition. The obtained results from Atlas and Mixed-Mode simulations are well in accordance with the results obtained from the analytical modeling. The inset shows the 3D schematic view of the photodetector. (b) The JlightV characteristics of the photodetector for different Pin at 77 K. (c) Jlight, Jlight/Jdark ratio, and linear dynamic range (LDR) of the photodetector as a function of Pin in self-powered mode (zero bias condition) at 77 K. The Jlight/Jdark ratio and LDR increases exponentially with Pin, whereas, Jlight increase linearly with Pin. (d) The variation of current densities, LDR, and (RA)NET with temperature at a bias of −1.0 V under illumination of 1 W cm−2. The current densities increase exponentially, whereas LDR and (RA)NET decreases with the increase in temperature due to the generation of thermally induced electron–hole pairs in addition to photoexcited carriers.

The JlightV characteristics under illumination at 20.6 µm for different Pin varying from 1 mW cm−2 to 2 W cm−2 are shown in Fig. 3b. The Jlight increases with the incident power, and shifts towards the positive voltage region due to unidirectional charge transport mechanism. The two important figure-of-merits to evaluate the electrical performance of photodetectors are Jlight/Jdark ratio and linear dynamic range33 (LDR (dB) = 20[thin space (1/6-em)]log(Jlight/Jdark)). Fig. 3c shows the Jlight, Jlight/Jdark ratio, and LDR for various Pin values at zero-bias and 77 K. The device exhibits Jlight/Jdark ratio of 4.8 × 1014 and LDR of 293.55 dB at 2 W cm−2 in self-powered mode and are better than that of Gr–Si based heterojunction photodetector.84,85 The photocurrent density Jlight and incident power Pin satisfy the relationship86 JlightPinα, where α is an empirical value related to the recombination process of the photoexcited carriers. From Fig. 3c, α = 1.0 is obtained for reverse biases varying from −1.0 to 0.0 V. The linear response of photocurrent density as a function of incident power indicates that the recombination loss is negligible for the proposed heterojunction photodetector. Fig. 3d shows the current density, LDR, and effective or net resistance area product (RA)NET with respect to temperature variation at a bias of −1.0 V and incident power of 1 W cm−2. The increase in temperature decreases the resistance and LDR, whereas, increases the current density. The (RA)NET arises due to different current densities, i.e., JDIFF, JGR, JTAT and JBTB, and can be written as:

 
image file: c8ra07683a-t35.tif(14)

The simulated and analytical resistance area product of the proposed photodetector for different voltages varying from −1.0 to 0.3 V at 77 K is shown in Fig. 3a. The photodetector exhibits a resistance area product image file: c8ra07683a-t15.tif of 0.3 MΩ cm2 in self-powered mode which in turn results in high specific detectivity.

Optical characterization

The optical analysis of proposed photodetector is performed by coupling the optical and basic semiconductor equations. The optical absorption coefficient of n-Hg1−xCdxTe material within the Kane region is calculated by Chu's empirical relation.87,88 For the photon energy Ep < Egn (tail region) and Ep > Egn (Kane region), the absorption coefficient is approximated by:
 
image file: c8ra07683a-t16.tif(15)
where α0 = e(−18.5+45.68x); E0 = −0.355 + 1.77x the fitting parameters which vary with x composition and
 
image file: c8ra07683a-t17.tif(16)
Here,
 
αg(x,T) = −65 + 1.88T + (8694 − 10.314T)x (17)
 
β(x,T) = −1 + 0.083T + (21 − 0.13T)x (18)

In order to compute the optical characteristics, complex refractive indices are described for both the BLG and MCT. The wavelength (λ) dependent complex refractive index for Gr is calculated by42 nGr(λ) = 3.0 + i1.8153λ, whereas, absorption coefficient is approximated by αp+(λ) = 1.8153 × 4π/λ. The complex refractive index of MCT as a function of x composition and temperature is given as:89

 
image file: c8ra07683a-t18.tif(19)
where
 
image file: c8ra07683a-t19.tif(20)

The imaginary part of the refractive index for MCT depends on the wavelength and absorption as.24 K = λαn(λ)/4π.

The spectral response of the proposed photodetector as a function of wavelength is shown in Fig. S1. The quantum efficiency (QE), photocurrent responsivity (Ri), specific detectivity (D*), and noise equivalent power (NEP) of proposed photodetector are evaluated using computer simulations. The two types of quantum efficiencies, i.e. internal QE (QEint) and external QE (QEext) are often considered for a photodetector. The QEint determines the internal photocurrent responsivity (Rinti), whereas QEext gives the external photocurrent responsivity (Rexti). The QEext, Rexti, D*, and NEP of the device are further evaluated using the analytical model. The QEext measures the wavelength dependent gain of the photodetector and can be given as32

 
image file: c8ra07683a-t20.tif(21)
where CM represents the hot carrier multiplication factor69–74 which is a function of bias voltage and ambient temperature, c is the speed of light, Jλ is the photocurrent density, and λ represents the wavelength of the incident radiation.

The net QEext of the photodetector comprises of neutral p+-(QEext)p+, neutral n-(QEext)n, and the depletion (QEext)dep regions, and can be written as:24,90–92

 
QEext = CM(V,T) × ((QEext)p+ + (QEext)n + (QEext)dep) (22)
where
 
image file: c8ra07683a-t21.tif(23)
 
image file: c8ra07683a-t22.tif(24)
and
 
image file: c8ra07683a-t23.tif(25)
Here, Rp+ and Rn are the Fresnel reflection coefficients at the entrance and p+–n interfaces, respectively.

The photocurrent responsivity is a ratio of photocurrent to the incident light power, whereas, quantum efficiency measures the sensitivity of the photodetector. On the other hand, the specific detectivity describes the smallest signal that a photodetector can detect, however, noise equivalent power is the minimum incident signal that a photodetector can resolve from the noise. The QEint of the IPE process is the number of carriers emitted to HgCdTe per absorbed photon, and QEext is the number of carriers emitted to HgCdTe per incident photon. The Rinti, Rexti, D*, and NEP are calculated using following relations:3,24,32,33,93

 
image file: c8ra07683a-t24.tif(26a)
 
image file: c8ra07683a-t25.tif(26b)
 
image file: c8ra07683a-t26.tif(27)
 
image file: c8ra07683a-t27.tif(28)
where Δf and A are the bandwidth, and active area, respectively. Here, NEP is estimated at a unity bandwidth, i.e. Δf = 1 Hz.

Fig. 4a shows the variation of QEext, Rexti, and NEP for the proposed photodetector as a function of wavelength at a of −0.5 V and a radiation of 1 W cm−2 at 20.6 µm and 77 K. The device exhibits a high QEint ∼ 99.49% (Fig. S1b), QEext ∼ 89%, Rinti ∼ 13.26 A W−1 (Fig. S1b), Rexti ∼ 9.1 A W−1, D* ∼ 7.6 × 1013 cm Hz1/2 W−1 (Fig. S2a), and low value of NEP ∼ 8.3 × 10−18 W.


image file: c8ra07683a-f4.tif
Fig. 4 The optical characteristics of p+-BLG/n-Hg0.8133Cd0.1867Te photodetector at a cut-off wavelength (λc) of 20.6 µm. (a) The external quantum efficiency (QEext), external photocurrent responsivity, (Rexti) and noise equivalent power (NEP) as a function of wavelength with Pin = 1 W cm−2, V = −0.5 V at 77 K. The results are well in accordance with the results obtained from analytical modeling. (b) The QEext(max), Rexti(max), and NEP(min) as a function of bias voltage with Pin = 1 W cm−2 at 77 K. The QEext(max) and, Rexti(max) increases with the bias voltage, whereas NEP(min) decreases with the applied bias. (c) The QEext(max), Rexti(max), and NEP(min) of the photodetector at 77 K under different Pin values with V = −0.5 V. The QEext(max) and NEP(min) decreases with Pin, whereas Rexti(max), increases with the increase in Pin. (d) The variation of QEext(max), Rexti(max), and NEP(min) with temperature under −0.5 V bias at 1 W cm−2. The QEext(max) and, Rexti(max) both increases with the increase in temperature, whereas NEP(min) initially increases upto 150 K and improves thereafter.

The influence of reverse bias voltage, incident power intensity, and temperature on the maximum external quantum efficiency (QEext(max)), maximum external photocurrent responsivity, Rexti(max) and minimum NEP (NEP(min)) under IR illumination are shown in Fig. 4b–d, respectively. The increase in reverse bias in Fig. 4b, increases the QEext(max), and Rexti(max) resulting in a lower NEP. The increase in both QEext(max), and Rexti(max) with the reverse bias voltage is mainly due to the increased drift velocity of the photo-induced charge carriers along with the increased probability of exciton separation and acceleration with the bias voltage, which eventually contribute to the total photocurrent in the external circuit. The increase in QEext is attributed to the carriers passing thin depletion region multiple times at a certain reverse bias.32 Fig. 4c demonstrates the variation of incident power suggesting increase in Rexti due to the increase in photocurrent which decreases both QEext and NEP. The decrease in QEext with incident power could also be attributed due to the self-induced-heating increase in the carrier scattering and hence the rate of charge carrier recombination. Furthermore, the increase in reverse bias and incident power results in improved D* as shown in Fig. S2b and c, respectively.

The effect of temperature variation on optical parameters of the device is shown in Fig. 4d. The QEext(max) increases from 10.68 to 3337.70%, whereas the Rexti(max) increases from 0.51 to 62.36 A/W for the temperatures varying from 30 to 250 K. The maximum D* image file: c8ra07683a-t28.tif changes from 3.8 × 1015 to 8.08 × 1012 cm Hz1/2 W−1 for temperatures 30–180 K, and from 3.04 × 1011 to 1.29 × 1013 cm Hz1/2 W−1 for the temperature range 200–250 K (see Fig. S2d). Accordingly, NEP(min) varies from 1.66 × 10−19 to 4.90 × 10−17 W for the temperature range 30–250 K as shown in Fig. 4d. The proposed photodetector demonstrates a QEext(max), Rexti(max), image file: c8ra07683a-t29.tif and NEP(min) of 3337.70%, 62.36 A W−1, 1.29 × 1013 cm Hz1/2 W−1 and 4.90 × 10−17 W, respectively, at near room temperature.

The high values of QEext more than 100% are generally associated with the well-known carrier multiplication effect in graphene.69–74 Such multiple hot-carrier generation can be explained with the schematic representation of energy band diagram of proposed device as shown in Fig. 5a. The incident optical energy excites an electron in the valence band to the higher conduction state of the graphene which further excites another valence band electron to conduction band as shown in Fig. 5a. Therefore, generation of multiple hot-carriers in graphene with single incident photon is due to impact ionization. Such carrier multiplication effect is observed to be increasing with doping in graphene.74 Moreover, under the illumination of high optical energy, light can also be absorbed in both the M- and K-points of the Brillouin zone in graphene resulting in enhanced carrier multiplication effect.33


image file: c8ra07683a-f5.tif
Fig. 5 (a) The energy band diagram of p+-BLG/n-Hg0.8133Cd0.1867Te heterojunction based VLWIR photodetector under illumination and reverse bias condition showing carrier multiplication (CM). (b) The carrier multiplication factor as a function of temperature at −0.5 and −1.0 V under illumination of 1 W cm−2. The CM factor increases exponentially with the increase in temperature.

The combined effect of carrier multiplication (in graphene) and presence of high electric field across the junction causes transport of multiple electrons (holes) to the positive (negative) bias electrodes which finally contributes to the net enhanced photocurrent and QEext.

The CM(V,T) can be estimated from the simulated JV characteristics under dark and illumination conditions at different temperatures as:27

 
image file: c8ra07683a-t30.tif(29)

Fig. 5b shows the estimated CM factor at −0.5 and −1.0 V bias as a function of temperature. The CM factor is observed to be increasing with ambient temperature exponentially which is attributed to the temperature dependence of the semiconductor current according to eqn (29). The CM factor is observed to be varying in the range of 1.05–1.24 and 1.06–1.25 at −0.5 and −1.0 V, respectively, for the temperature range 77 to 250 K. With increasing reverse bias, the probability of carrier recombination decreases resulting in long life-time of photo-generated carriers and, hence, improves effective carrier multiplication in the device. In our case, the obtained values of hot CM factor for p+-doped graphene are well in accordance with the previously reported experimental values.73,74

The variation of QEext as a function of photon energy is shown in Fig. 6. The QEext increases with the incident photon energy due to prominent hot CM under illumination with higher energy than the band-gap of BLG. On the other hand, photon energy smaller than the BLG band-gap lowers the QEext which is attributed to the decreased carrier multiplication as shown in Fig. 6. Furthermore, the external reverse bias provides a high electric field to the device which increases the probability of electron–hole pair separation and enhances drift-velocity of the photogenerated charge carriers in both graphene and MCT.


image file: c8ra07683a-f6.tif
Fig. 6 The QEext as a function of photon energy with an incident power of 1 W cm−2 at −0.5 V bias for different temperatures varying from 30 to 250 K. The QEext exceeds 100% due to the generation of long lifetime of photo-induced hot carriers in VLWIR region.

In addition, we have estimated the shot (quantum) and Johnson–Nyquist (thermal) noise,93 which also dominate in the photodetector. Accordingly, the shot (is) and Johnson–Nyquist (ij) noise currents are calculated by82 image file: c8ra07683a-t31.tif and image file: c8ra07683a-t32.tif, where Idark is the dark current RNET = (dI/dV)−1, is the net resistance of photodetector in dark condition at reverse bias and Δf = 1 Hz is the bandwidth. The total noise current (in)93 and SNR82 are given by in = is + ij and image file: c8ra07683a-t33.tif

The estimated values of in and SNR are 1.06 fA and 156.18 dB, respectively, for −0.5 V bias and a radiation of 1 W cm−2 at 20.6 µm and 77 K. Fig. 7 shows the 3 dB cut-off frequency (f3 dB) and response time (tr) as a function of temperature at −0.5 V bias with incident power of 1 W cm−2. Beyond 3 dB cut-off frequency, the current/gain starts rolling-off quickly. The response time suggests the increase in output signal from 10–90% of the maximum value and is related to 3 dB cut-off as85

 
image file: c8ra07683a-t34.tif(30)


image file: c8ra07683a-f7.tif
Fig. 7 The f3 dB and tr as a function of temperature with V = −0.5 V and Pin = 1 W cm−2. The f3 dB rise exponentially with temperature, whereas, tr decay exponentially with temperature, due to increase in depletion length at higher temperatures which in turn reduces space-charge capacitance.

The results suggest exponential increase in 3 dB cut-off frequency from 3.89 to 129 GHz due to the existence of high saturation velocity and high carrier mobility, whereas tr decreases from 87.4 to 2.6 ps as shown in Fig. 7. The reduction in depletion (space-charge) capacitance and increase in depletion length is responsible for obtaining larger cut-off frequency.82 It can be further increased with the increase in reverse bias voltage and reduction in the device active area inducing reduced capacitance. To the best of our knowledge, the obtained results for the proposed photodetector are better than that of previously reported graphene based photodetectors.1,3,29,30,33,37,39,43,82–85,93–103 Table 2 summarizes the key parameters of our proposed device with other MCT and graphene based photodetectors reported earlier.

Table 2 Performance comparison of proposed device with other graphene and MCT based photodetectors reported earlier
  Device structure QE (%) Ri (A W−1) D* (cm Hz1/2 W−1) NEP (W Hz−1/2) Jlight/Jdark tr f3 dB LDR (dB) Ref.
Experimental Study Graphene/Si Schottky junction QEint = 10–30 0.0028–0.0099 M. Amirmazlaghani et al.1
Graphene/Ge Schottky junction 0.00518 1.38 × 1010 2 × 104 23 µs L. H. Zeng et al.3
BLG terahertz photodetector 9 × 106 M. Mohammadian et al.29
Gr/SiO2/Si photodetector Qint = 6–16 0.0005 106 GHz F. Xia et al.30
Graphene/silicon Schottky junction ∼98 0.2 1.6 × 1013 1.2 × 106 119 X. Wan et al.33
Graphene nanoribbons passivated with HfO2 1.75, 1.5 and 0.18 ∼7 ± 1 X. Yu et al.37
BLG/GaAs Schottky junction 0.0012 7.3 × 109 1.2 × 103 32 µs L. B. Luo et al.39
BLG/GaAs Schottky junction with AlOx interface passivation layer 0.005 2.88 × 1011 3 × 105 320 ns L. B. Luo et al.39
Multilayer armchair graphene nanoribbons 2.1 × 1011 at 77 K and 2.2 × 108 at 300 K E. Ahmadi et al.83
Graphene/silicon heterojunction QEext = 60 0.73 4.2 × 1012 0.075 × 10−12 107 320 µs X. Li et al.84
Graphene/Si with interfacial oxide layer QEext = 60 0.73 5.77 × 1013 0.0055 × 10−12 107 320 µs 90 X. Li et al.84
Graphene/silicon Schottky junction QEext = 60–70 0.0003 12 ns 2.5 MHz H. Selvi et al.85
Graphene/silicon Schottky junction Rinti = 0.25 Rexti = 0.02 120 MHz M. Casalino et al.93
HgCdTe multilayer heterostructure 8.5 1.6 × 109 0.1 GHz M. Kopytko et al.94
GaAs nanocone/MLG array Schottky junction 0.00373 1.83 × 1011 104 72 µs L. B. Luo et al.95
All-carbon graphene nanoribbon-C60 hybrid nanostructure 0.4 4 s X. Yu et al.96
Graphene nanowalls/Si heterojunction 0.52 5.88 × 1013 5.96 × 10−15 2 × 107 40 µs 8.5 kHz J. Shen et al.97
Graphene/Bi2Se3 heterostructure 8.18 1.7 × 109 J. Kim et al.98
Graphene/silicon heterojunction QEint = 65 0.435 7.69 × 109 1 × 10−12 104 1.2 ms X. An et al.99
MLG/InP Schottky junction 3.96 0.0461 3.62 × 109 3.75 × 10−12 230 25.9 µs 9.2 kHz 51.7 L. B. Luo et al.100
MLG/InP with SiO2 encapsulated gold nanorods 14.7 0.1398 10.5 × 1010 776 441 ns 104 kHz L. B. Luo et al.100
Theoretical/simulation study HgCdTe based heterojunction 78 at 77 K 4.7 × 1012 at 77 K 2 × 10−12 at 1 Hz and 77 K P. K. Saxena et al.23
HgCdTe based heterojunction 80 at 77 K 6.75 at 77 K 2.25 × 109 at 77 K 1 × 10−17 at 1 Hz and 77 K A. D. D. Dwivedi24
Multiple graphene layer photodetectors 12 for MLG; 35–350 for 50 layers graphene (4.1–8.2) × 108 for MLG at 300 K; (1.7–3.4) × 109 for 50 layers graphene at 300 K; (1.7–3.4) × 1013 for 50 layers graphene at 77 K V. Ryzhii et al.43
Multiple graphene layer photodetectors 4.6 for MLG; 1.8 for 100 layers graphene 227 for 100 layers graphene 109 at 300 K M. Ryzhii et al.44
HgCdTe based homojunction 67 at 77 K 1 × 10−13 at 1 Hz and 77 K P. K. Saxena et al.82
MLG photodetector QEint = 2.5–10.2 8.4 × 10−4-3.4 × 10−3 Q. Gao et al.101
Multiple graphene layer photodetectors 4.6 for MLG; 74 for 20 layers graphene 1.8 for 100 layers graphene 227 for 100 layers graphene 1013 at 77 K 109 at 300 K V. Ryzhii et al.102
Graphene superlattice-based photodetector 20 0.866 M. Moradinasab et al.103
p+-BLG/n-HgCdTe heterojunction QEint = 99.49% QEext = 89 at 77 K QEext = 3337.70 at 250 K Rinti = 13.36 Rexti = 9.1 at 77 K, Rexti = 62.36 at 250 K 7.6 × 1013 at 77 K1.29 × 1013 at 250 K 8.3 × 10−18 at 77 K and 1 Hz 4.90 × 10−17 W at 250 K and 1 Hz 4.8 × 1014 9.4 ps at 77 K 2.6 ps at 250 K 36.16 GHz at 77 K 129 GHz at 250 K 293.55 Present work


Conclusions

In summary, we have demonstrated a high-performance p+-BLG and few layer graphene/n-Hg0.8133Cd0.1867Te heterojunction VLWIR photodetector. The various electrical and optical characteristic parameters are computed and analysed using computer simulations and are further validated by an analytical model based on drift-diffusion, tunneling and Chu's methods. The dark current density is reduced due to lower thermo-generation rate of BLG and MCT heterostructure, offering the high quantum efficiency, high photocurrent responsivity, high specific detectivity, low noise equivalent power, low noise current, and better signal to noise ratio. The near room temperature external quantum efficiency of 3337.70% and responsivity of 62.36 A W−1 at −0.5 V bias are achieved in addition to a higher 3 dB cut-off frequency (∼129 GHz) and short response time (∼2.6 ps). Such superior performances are obtained due to hot carrier multiplication mechanism in graphene. The obtained results suggest the utilisation of p+-BLG/n-Hg0.8133Cd0.1867Te heterostructure for next-generation high-performance, ultra-low-power, low noise, and cost effective IR photodetection.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

Authors would like to thank P. K. Saxena at Technext Lab (P) Limited, Lucknow; A. D. D. Dwivedi at Poornima University, Jaipur; and A. Das at University of Calcutta, Kolkata, India for technical discussions.

References

  1. M. Amirmazlaghani, F. Raissi, O. Habibpour, J. Vukusic and J. Stake, IEEE J. Quantum Electron., 2013, 49, 589–594 CAS.
  2. S. Assefa, F. Xia and Y. A. Vlasov, Nature, 2010, 464, 80–84 CrossRef CAS PubMed.
  3. L. H. Zeng, M. Z. Wang, H. Hu, B. Nie, Y. Q. Yu, C. Y. Wu, L. Wang, J. G. Hu, C. Xie, F. X. Liang and L. B. Luo, ACS Appl. Mater. Interfaces, 2013, 5, 9362–9366 CrossRef CAS PubMed.
  4. A. Rogalski, Prog. Quantum Electron., 2003, 27, 59–210 CrossRef CAS.
  5. J. Yoon, S. Jo, I. S. Chun, I. Jung, H. S. Kim, M. Meitl, E. Menard, X. Li, J. J. Coleman, U. Paik and J. A. Rogers, Nature, 2010, 465, 329–333 CrossRef CAS PubMed.
  6. J. Miao, W. Hu, N. Guo, Z. Lu, X. Liu, L. Liao, P. Chen, T. Jiang, S. Wu, J. C. Ho, L. Wang, X. Chen and W. Lu, Small, 2015, 11, 936–942 CrossRef CAS PubMed.
  7. P. Norton, Opto-Electron. Rev., 2002, 10, 159–174 CAS.
  8. A. Rogalski, J. Alloys Compd., 2004, 371, 53–57 CrossRef CAS.
  9. J. Wang, X. Chen, W. Hu, L. Wang, W. Lu, F. Xu, J. Zhao, Y. Shi and R. Ji, Appl. Phys. Lett., 2011, 99, 113508 CrossRef.
  10. P. S. Wijewarnasuriya, Y. Chen, G. Brill, B. Zandi and N. K. Dhar, IEEE Trans. Electron Devices, 2010, 57, 782–787 CAS.
  11. N. Liu, H. Tian, G. Schwartz, J. B. H. Tok, T. L. Ren and Z. Bao, Nano Lett., 2014, 14, 3702–3708 CrossRef CAS PubMed.
  12. A. Rogalski, Rep. Prog. Phys., 2005, 68, 2267–2336 CrossRef CAS.
  13. V. Ryzhii and M. Ryzhii, Phys. Rev. B: Condens. Matter Mater. Phys., 2009, 79, 245311 CrossRef.
  14. P. K. Saxena, Infrared Phys. Technol., 2011, 54, 25–33 CrossRef CAS.
  15. P. K. Saxena, Def. Sci. J., 2017, 67, 141–148 CrossRef.
  16. A. Rogalski and P. Martyniuk, Infrared Phys. Technol., 2006, 48, 39–52 CrossRef CAS.
  17. B. F. Levine, K. K. Choi, C. G. Bethea, J. Walker and R. J. Malik, Appl. Phys. Lett., 1987, 50, 1092–1094 CrossRef CAS.
  18. A. Asgari and S. Razi, Opt. Express, 2010, 18, 14604–14615 CrossRef CAS PubMed.
  19. A. Asgari, E. Ahmadi and M. Kalafi, Microelectron. J., 2009, 40, 104–107 CrossRef CAS.
  20. S. Bansal, K. Sharma, N. Gupta and A. K. Singh, in 2016 IEEE Uttar Pradesh Section International Conference on Electrical, Computer and Electronics Engineering, UPCON 2016, 2016, pp. 422–425 Search PubMed.
  21. M. Kopytko, A. Keblowski, W. Gawron, A. Kowalewski and A. Rogalski, IEEE Trans. Electron Devices, 2014, 61, 3803–3807 CAS.
  22. N. D. Akhavan, G. A. Umana-membreno, R. Gu, J. Antoszewski and L. Faraone, IEEE Trans. Electron Devices, 2018, 65, 591–598 CAS.
  23. P. K. Saxena and P. Chakrabarti, Infrared Phys. Technol., 2009, 52, 196–203 CrossRef CAS.
  24. A. D. D. Dwivedi, J. Appl. Phys., 2011, 110, 43101 CrossRef.
  25. S. Bansal, K. Sharma, K. Soni, N. Gupta and A. K Singh, in 2017 Progress In Electromagnetics Research Symposium-Spring, PIERS, St Petersburg, Russia, 2017, pp. 981–983 Search PubMed.
  26. E. Bellotti and D. D'Orsogna, IEEE J. Quantum Electron., 2006, 42, 418–426 CrossRef CAS.
  27. A. Singh, A. K. Shukla and R. Pal, IEEE Trans. Electron Devices, 2017, 64, 1146–1152 Search PubMed.
  28. A. Piotrowski, P. Madejczyk, W. Gawron, K. Kłos, J. Pawluczyk, J. Rutkowski, J. Piotrowski and A. Rogalski, Infrared Phys. Technol., 2007, 49, 173–182 CrossRef CAS.
  29. M. Mohammadian and H. R. Saghai, Optik, 2015, 126, 1156–1160 CrossRef CAS.
  30. F. Xia, T. Mueller, Y. M. Lin, A. V. Garcia and P. Avouris, Nat. Nanotechnol., 2009, 4, 839–843 CrossRef CAS PubMed.
  31. B. Nie, J. G. Hu, L. B. Luo, C. Xie, L. H. Zeng, P. Lv, F. Z. Li, J. S. Jie, M. Feng, C. Y. Wu, Y. Q. Yu and S. H. Yu, Small, 2013, 9, 2872–2879 CrossRef CAS PubMed.
  32. S. Dhar, T. Majumder and S. P. Mondal, ACS Appl. Mater. Interfaces, 2016, 8, 31822–31831 CrossRef CAS PubMed.
  33. X. Wan, Y. Xu, H. Guo, K. Shehzad, A. Ali, Y. Liu, J. Yang, D. Dai, C.-T. Lin, L. Liu, H.-C. Cheng, F. Wang, X. Wang, H. Lu, W. Hu, X. Pi, Y. Dan, J. Luo, T. Hasan, X. Duan, X. Li, J. Xu, D. Yang, T. Ren and B. Yu, NPJ 2D Mater. Appl., 2017, 1, 1–8 CrossRef.
  34. D. Spirito, S. Kudera, V. Miseikis, C. Giansante, C. Coletti and R. Krahne, J. Phys. Chem. C, 2015, 119, 23859–23864 CrossRef CAS.
  35. Z. Gao, W. Jin, Y. Zhou, Y. Dai, B. Yu, C. Liu, W. Xu, Y. Li, H. Peng, Z. Liu and L. Dai, Nanoscale, 2013, 5, 5576–5581 RSC.
  36. F. Lin, S. W. Chen, J. Meng, G. Tse, X. W. Fu, F. J. Xu, B. Shen, Z. M. Liao and D. P. Yu, Appl. Phys. Lett., 2014, 105, 73103 CrossRef.
  37. X. Yu, Z. Dong, Y. Liu, T. Liu, J. Tao, Y. Zeng, J. K. W. Yang and Q. J. Wang, Nanoscale, 2016, 8, 327–332 RSC.
  38. Z. Sun, Z. Liu, J. Li, G. A. Tai, S. P. Lau and F. Yan, Adv. Mater., 2012, 24, 5878–5883 CrossRef CAS PubMed.
  39. L. B. Luo, H. Hu, X.-H. Wang, R. Lu, Y.-F. Zou, Y.-Q. Yu and F.-X. Liang, J. Mater. Chem. C, 2015, 3, 4723–4728 RSC.
  40. T. Mueller, F. Xia and P. Avouris, Nat. Photonics, 2010, 4, 297–301 CrossRef CAS.
  41. X. Gan, R. J. Shiue, Y. Gao, I. Meric, T. F. Heinz, K. Shepard, J. Hone, S. Assefa and D. Englund, Nat. Photonics, 2013, 7, 883–887 CrossRef CAS.
  42. A. Pospischil, M. Humer, M. M. Furchi, D. Bachmann, R. Guider, T. Fromherz and T. Mueller, Nat. Photonics, 2013, 7, 892–896 CrossRef CAS.
  43. V. Ryzhii, M. Ryzhii, V. Mitin and T. Otsuji, J. Appl. Phys., 2010, 107, 54512 CrossRef.
  44. M. Ryzhii, T. Otsuji, V. Mitin and V. Ryzhii, Jpn. J. Appl. Phys., 2011, 50, 70117 CrossRef.
  45. G. Konstantatos, M. Badioli, L. Gaudreau, J. Osmond, M. Bernechea, F. P. G. De Arquer, F. Gatti and F. H. L. Koppens, Nat. Nanotechnol., 2012, 7, 363–368 CrossRef CAS PubMed.
  46. M. Pykal, P. Jurečka, F. Karlický and M. Otyepka, Phys. Chem. Chem. Phys., 2016, 18, 6351–6372 RSC.
  47. S. Zhao and J. Xue, Phys. Rev. B, 2012, 86, 1–10 Search PubMed.
  48. P. A. Denis, Chem. Phys. Lett., 2010, 492, 251–257 CrossRef CAS.
  49. W. Xu, Y. Gong, L. Liu, H. Qin and Y. Shi, Nanoscale Res. Lett., 2011, 6, 250 CrossRef PubMed.
  50. S. Bae, H. Kim, Y. Lee, X. F. Xu, J. S. Park, Y. Zheng, J. Balakrishnan, T. Lei, H. R. Kim, Y. I. Song, Y. J. Kim, K. S. Kim, B. Ozyilmaz, J. H. Ahn, B. H. Hong and S. Iijima, Nat. Nanotechnol., 2010, 5, 574–578 CrossRef CAS PubMed.
  51. A. Kasry, M. A. Kuroda, G. J. Martyna, G. S. Tulevski and A. A. Bol, ACS Nano, 2010, 4, 3839–3844 CrossRef CAS PubMed.
  52. I. Khrapach, F. Withers, T. H. Bointon, D. K. Polyushkin, W. L. Barnes, S. Russo and M. F. Craciun, Adv. Mater., 2012, 24, 2844–2849 CrossRef CAS PubMed.
  53. Y. M. Shi, K. K. Kim, A. Reina, M. Hofmann, L. J. Li and J. Kong, ACS Nano, 2010, 4, 2689–2694 CrossRef CAS PubMed.
  54. K. K. Kim, A. Reina, Y. M. Shi, H. Park, L. J. Li, Y. H. Lee and J. Kong, Nanotechnology, 2010, 21, 285205 CrossRef PubMed.
  55. V. C. Tung, L. M. Chen, M. J. Allen, J. K. Wassei, K. Nelson, R. B. Kaner and Y. Yang, Nano Lett., 2009, 9, 1949–1955 CrossRef CAS PubMed.
  56. J. K. Wassei, K. C. Cha, V. C. Tung, Y. Yang and R. B. Kaner, J. Mater. Chem., 2011, 21, 3391–3396 RSC.
  57. X. Meng, S. Tongay, J. Kang, Z. Chen, F. Wu, S. S. Li, J. B. Xia, J. Li and J. Wu, Carbon, 2013, 57, 507–514 CrossRef CAS.
  58. L. Tai, D. Zhu, X. Liu, T. Yang, L. Wang, R. Wang, S. Jiang, Z. Chen, Z. Xu and X. Li, Nano-Micro Lett., 2018, 10, 1–9 CrossRef PubMed.
  59. K. S. Novoselov, D. Jiang, F. Schedin, T. J. Booth, V. V. Khotkevich, S. V. Morozov and A. K. Geim, PNAS, 2005, 102, 10451–10453 CrossRef CAS PubMed.
  60. W. Jung, J. Park, T. Yoon, T. S. Kim, S. Kim and C. S. Han, Small, 2014, 10, 1704–1711 CrossRef CAS PubMed.
  61. C. J. Shearer, A. D. Slattery, A. J. Stapleton, J. G. Shapter and C. T. Gibson, Nanotechnology, 2016, 27, 125704 CrossRef PubMed.
  62. R. Quhe, J. Ma, Z. Zeng, K. Tang, J. Zheng, Y. Wang, Z. Ni, L. Wang, Z. Gao, J. Shi and J. Lu, Sci. Rep., 2013, 3, 1–8 Search PubMed.
  63. F. Xia, D. B. Farmer, Y.-M. Lin and P. Avouris, Nano Lett., 2010, 10, 715–718 CrossRef CAS PubMed.
  64. A. Suhail, G. Pan, D. Jenkins and K. Islam, Carbon, 2018, 129, 520–526 CrossRef CAS.
  65. F. H. L. Koppens, T. Mueller, P. Avouris, A. C. Ferrari, M. S. Vitiello and M. Polini, Nat. Nanotechnol., 2014, 9, 780–793 CrossRef CAS PubMed.
  66. J. Liu, Y. Yin, L. Yu, Y. Shi, D. Liang and D. Dai, Sci. Rep., 2017, 7, 1–7 CrossRef PubMed.
  67. K. Patel and P. K. Tyagi, Carbon, 2017, 116, 744–752 CrossRef CAS.
  68. W. W. Anderson, Infrared Phys., 1980, 20, 363–372 CrossRef CAS.
  69. Y. Zhang, T. Liu, B. Meng, X. Li, G. Liang, X. Hu and Q. J. Wang, Nat. Commun., 2013, 4, 1811 CrossRef PubMed.
  70. K. J. Tielrooij, J. C. W. Song, S. A. Jensen, A. Centeno, A. Pesquera, A. Zurutuza Elorza, M. Bonn, L. S. Levitov and F. H. L. Koppens, Nat. Phys., 2013, 9, 248–252 Search PubMed.
  71. Y. K. Lee, H. Choi, H. Lee, C. Lee, J. S. Choi, C. G. Choi, E. Hwang and J. Y. Park, Sci. Rep., 2016, 6, 1–9 Search PubMed.
  72. T. Plötzing, T. Winzer, E. Malic, D. Neumaier, A. Knorr and H. Kurz, Nano Lett., 2014, 14, 5371–5375 CrossRef PubMed.
  73. J. C. Johannsen, S. Ulstrup, A. Crepaldi, F. Cilento, M. Zacchigna, J. A. Miwa, C. Cacho, R. T. Chapman, E. Springate, F. Fromm, C. Raidel, T. Seyller, P. D. C. King, F. Parmigiani, M. Grioni and P. Hofmann, Nano Lett., 2015, 15, 326–331 CrossRef CAS PubMed.
  74. F. Kadi, T. Winzer, A. Knorr and E. Malic, Sci. Rep., 2015, 5, 1–7 Search PubMed.
  75. T. Winzer, A. Knorr and E. Malic, Nano Lett., 2010, 10, 4839–4843 CrossRef CAS PubMed.
  76. C. O. Kim, S. Kim, D. H. Shin, S. S. Kang, J. M. Kim, C. W. Jang, S. S. Joo, J. S. Lee, J. H. Kim, S. H. Choi and E. Hwang, Nat. Commun., 2014, 5, 3249 CrossRef PubMed.
  77. M. G. Ancona, IEEE Trans. Electron Devices, 2010, 57, 681–689 CAS.
  78. A. D. D. Dwivedi and P. Chakrabarti, Opt. Quantum Electron., 2007, 39, 627–641 CrossRef CAS.
  79. ATLAS User's Manual Version 5.20.2.R, SILVACO International, Santa Clara, CA 95054, 2016 Search PubMed.
  80. M. H. Weiler, Semicond. Semimetals, 1981, 16, 119–191 CAS.
  81. K. Patel and P. K. Tyagi, AIP Adv., 2015, 5, 077165 CrossRef.
  82. P. K. Saxena and P. Chakrabarti, Optoelectron. Adv. Mater., Rapid Commun., 2008, 2, 140–147 CAS.
  83. E. Ahmadi and A. Asgari, J. Appl. Phys., 2013, 113, 93106 CrossRef.
  84. X. Li, M. Zhu, M. Du, Z. Lv, L. Zhang, Y. Li, Y. Yang, T. Yang, X. Li, K. Wang, H. Zhu and Y. Fang, Small, 2016, 12, 595–601 CrossRef CAS PubMed.
  85. H. Selvi, N. Unsuree, E. Whittaker, M. Halsall, E. W. Hill, A. G. Thomas, P. Parkinson and T. Echtermeyer, Nanoscale, 2018, 10, 3399–3409 RSC.
  86. H. L. Zhu, W. C. H. Choy, W. E. I. Sha and X. Ren, Adv. Opt. Mater., 2014, 2, 1082–1089 CrossRef CAS.
  87. J. Chu, Z. Mi and D. Tang, J. Appl. Phys., 1992, 71, 3955–3961 CrossRef CAS.
  88. J. Chu, B. Li, K. Liu and D. Tang, J. Appl. Phys., 1994, 75, 1234–1235 CrossRef CAS.
  89. K. Liu, J. H. Chu and D. Y. Tang, J. Appl. Phys., 1994, 75, 4176–4179 CrossRef CAS.
  90. A. Rogalski, Infrared Detectors, CRC Press, 2nd edn, 2010 Search PubMed.
  91. Y. Tian, B. Zhang, T. Zhan, H. Jiang and Y. Jin, IEEE Trans. Electron Devices, 2000, 47, 544–552 CrossRef CAS.
  92. P. Chakrabarti, A. Krier and A. F. Morgan, IEEE Trans. Electron Devices, 2003, 50, 2049–2058 CrossRef CAS.
  93. M. Casalino, U. Sassi, I. Goykhman, A. Eiden, E. Lidorikis, S. Milana, D. D. Fazio, F. Tomarchio, M. Iodice, G. Coppola and A. C. Ferrari, ACS Nano, 2017, 11, 10955–10963 CrossRef CAS PubMed.
  94. M. Kopytko, A. Kebłowski, P. Madejczyk, P. Martyniuk, J. Piotrowski, W. Gawron, K. Grodecki, K. Jozwikowski and J. Rutkowski, J. Electron. Mater., 2017, 46, 6045–6055 CrossRef CAS.
  95. L. B. Luo, J. J. Chen, M. Z. Wang, H. Hu, C. Y. Wu, Q. Li, L. Wang, J. A. Huang and F. X. Liang, Adv. Funct. Mater., 2014, 24, 2794–2800 CrossRef CAS.
  96. X. Yu, Z. Dong, J. K. W. Yang and Q. J. Wang, Optica, 2016, 3, 979–984 CrossRef.
  97. J. Shen, X. Liu, X. Song, X. Li, J. Wang, Q. Zhou, S. Luo, W. Feng, S. Lu, S. feng, X. Wei, C. Du, Y. Wang, H. Shi and D. Wei, Nanoscale, 2017, 9, 6020–6025 RSC.
  98. J. Kim, S. Park, H. Jang, N. Koirala, J. B. Lee, U. J. Kim, H. S. Lee, Y. G. Roh, H. Lee, S. Sim, S. Cha, C. In, J. Park, J. Lee, M. Noh, J. Moon, M. Salehi, J. Sung, S. S. Chee, M. H. Ham, M. H. Jo, S. Oh, J. H. Ahn, S. W. Hwang, D. Kim and H. Choi, ACS Photonics, 2017, 4, 482–488 CrossRef CAS.
  99. X. An, F. Liu, Y. J. Jung and S. Kar, Nano Lett., 2013, 13, 909–916 CrossRef CAS PubMed.
  100. L. B. Luo, Y. F. Zou, C. W. Ge, K. Zheng, D. D. Wang, R. Lu, T. F. Zhang, Y. Q. Yu and Z. Y. Guo, Adv. Opt. Mater., 2016, 4, 763–771 CrossRef CAS.
  101. Q. Gao and J. Guo, J. Appl. Phys., 2012, 112, 084316 CrossRef.
  102. V. Ryzhii, M. Ryzhii, N. Ryabova, V. Mitin and T. Otsuji, Infrared Phys. Technol., 2011, 54, 302–305 CrossRef CAS.
  103. M. Moradinasab, M. Pourfath, M. Fathipour and H Kosina, IEEE Trans. Electron Devices, 2015, 62, 593–600 CAS.

Footnote

Electronic supplementary information (ESI) available. See DOI: 10.1039/c8ra07683a

This journal is © The Royal Society of Chemistry 2018