Open Access Article
Qi Xun Xia
a,
Jianjian Fua,
Je Moon Yun
*b,
Rajaram S. Mane
b and
Kwang Ho Kim*ab
aSchool of Materials Science and Engineering, Pusan National University, San 30 Jangjeon-dong, Geumjeong-gu, Busan 609-735, Republic of Korea. E-mail: kwhokim@pusan.ac.kr
bGlobal Frontier R&D Center for Hybrid Interface Materials, Pusan National University, San 30 Jangjeon-dong, Geumjeong-gu, Busan 609-735, Republic of Korea. E-mail: yunjemoon@gmail.com
First published on 10th February 2017
A Ti3C2Tx MXene electrode decorated with NiO nanosheets was synthesized by a facile and cost-effective hydrothermal method. The NiO nanosheets were grown and immobilized on the carbon-supported TiO2 layer which was derived from Ti3C2Tx-MXene during a thermal annealing process. An electrode based on the NiO-grown derived-TiO2/C-Ti3C2Tx-MXene nanocomposite (Ni-dMXNC) exhibited a remarkable maximum specific capacity of 92.0 mA h cm−3 at 1 A g−1 and 53.9 mA h cm−3 at 10 A g−1. Furthermore, an asymmetric supercapacitor (ASC) device composed of Ni-dMXNC as the positive electrode and Ti3C2Tx MXene as the negative electrode was demonstrated to be better with a high energy density of 1.04 × 10−2 W h cm−3 at a power density of 0.22 W cm−3, and cycling stability with 72.1% retention after 5000 cycles, compared to ASCs using previously reported Ti3C2Tx MXene materials. The enhanced capacitive performance is attributed to the newly formed high-surface-area multilayers of the Ni-dMXNC architecture, the active surface of NiO layer, and a favourable synergetic behaviour of the Ti3C2Tx MXene negative electrode.
The MXene group of materials displays unusual combined metallic conductivity and hydrophobicity, excellent chemical, thermal, and environmental stabilities, and excellent mechanical properties,11,17 for which they are under investigation as anode materials in Li-ion batteries18,19 and supercapacitors.20,21 Supercapacitors are considered among the most promising energy storage devices because they have fast charge and discharge rates, high power densities, long cycle lifetimes, and greater reliability than Li-ion batteries.22–24 Rakhi et al. explored Ti3C2Tx MXene electrodes with the specific capacitance of 51 F g−1 in an electrolyte of 30 wt% KOH and a current density of 1 A g−1.25 Recently, Lin et al. reported on a 2D Ti3C2Tx MXene electrode with 117 F g−1 at a scan rate of 2 mV s−1 in 1 M KOH electrolyte.26 However, for the portable electronics and vehicles, the areal and volumetric performances are two important indicators for supercapacitors.27 The volumetric performance reflects how large and fast energy can be stored in a unit volume of materials/packed device, which indicates more reliable and precise parameter for evaluating the charge-storage capacity of supercapacitor compared with that of gravimetric performance.28,29 MXene electrode materials display significantly higher volumetric capacitances compared to previously reported carbon-based materials, which have capacitances limited to 60 F cm−3.30 The high packing density of MXenes described it as a promising electrode material for energy storage devices with high volumetric energy and power densities.31
In continuation of our ongoing positive and negative electrode materials research, in this work we have synthesized carbon-supported TiO2 on Ti3C2Tx MXene surface area, which called derived TiO2/C-Ti3C2Tx-MXene by an oxidation process. Compare with the Ti3C2Tx-MXene, the derived TiO2/C-Ti3C2Tx-MXene displaying higher conductivity and bigger specific surface area,32 which are of great importance and considered to be the key factors in improving the performance of supercapacitors. The derived TiO2/C-Ti3C2Tx-MXene electrodes decorated with NiO nanosheets, named derived TiO2/C-Ti3C2Tx-MXene/NiO nanocomposite (Ni-dMXNC) electrodes, and tested them as potential positive electrode materials. They demonstrated higher performances than previously reported MXenes.
In the MXene family, Ti3C2 is one of the lightest members. We selected Ti3C2 MXene as the basis for this contribution. The Ti3C2-based MXene powders were synthesized by etching Al from the Ti3AlC2 MAX phase. The as-obtained Ti3C2 surface was then terminated with functional groups, such as –OH,
O, and –F; for simplicity, in this text we utilize the chemical formula “Ti3C2Tx” to represent the as-produced surface-terminated MXene, where T represents the terminating groups and x is the number of groups per Ti3C2 unit cell. Herein, we report for the first time the superior electrochemical performance of a Ni-dMXNC//Ti3C2Tx MXene asymmetric supercapacitor (ASC) device relative to the previously reported symmetric supercapacitors (SSCs) with Ti3C2Tx MXene-based electrodes. This demonstrates the superiority of the composited Ti3C2Tx MXene in energy storage devices relative to Ti3C2Tx MXene alone; this superiority may be valid for other MXene materials too.
:
Al
:
C = 3
:
1
:
2 for 12 h in a planetary ball mill machine. Then the MAX, i.e. Ti3AlC2, as the precursor of the MXene Ti3C2Tx, was obtained through the chemical reaction| 3Ti + Al + 2C → Ti3AlC2 | (1) |
:
1
:
1. All were pasted to the 1 cm × 1 cm Ni foam area and pressed at 30 MPa. The electrode was then dried at 50 °C in vacuum for 12 h and used as an electrode in the rest of the measurements. To prepare the Ti3C2Tx MXene electrode, the same procedure was adopted, but except NiO. While monitoring the mass density of the Ni-dMXNC and Ti3C2Tx powders amounts of equal mass were cold-pressed into 10 mm-diameter separate thin discs under 30 MPa pressure.
![]() | (2) |
In order to observe the potential change of each electrode, a Ni-dMXNC material (positive electrode) and a Ti3C2Tx MXene material (negative electrode) were placed face-to-face and measured in 1 M KOH. The mass ratio of the active materials (Ni-dMXNC
:
Ti3C2Tx) was estimated to be 1
:
4.39. The GCD curves of asymmetric cells with the potential change of each individual electrode were monitored in situ by an auxiliary channel and a reference electrode (mercury/mercury oxide).35
:
Ti3C2Tx) was estimated at 1
:
4.39. The Ni-dMXNC and Ti3C2Tx MXene electrodes were separated with a cellulose paper separator. CR2032 coin-cell packaging was used in assembling the devices. An electrolyte of 1 M KOH was used, introduced over or into each electrode before fixing the coin cell for the ASC using a hydraulic coin-cell sealing machine (Shenzhen Pengxiangyunda Machinery, PX-HS-20). The specific discharge capacity (mA h g−1) of the ASC device (QD) was calculated from the GCD curves according to eqn (3),
![]() | (3) |
The energy density (W h cm−3) and power density (W cm−3) values of the Ni-dMXNC//Ti3C2Tx ASC, as derived from the GCD curves, were calculated using the following equations:34,36
![]() | (4) |
| V = mp/ρp + mn/ρn | (5) |
| P = E/Δt | (6) |
is the galvanostatic discharge current area, mp and mn is mass of positive and negative electrodes, ρp and ρn is the mass density of positive and negative electrodes, respectively. P (W cm−3) is the power density, and Δt (s) is the discharge time.
Side-view surface field-emission SEM (FESEM) images of the obtained Ti3AlC2 MAX phase and the Ti3C2Tx MXene are shown in Fig. S1 (ESI†). Fig. S1a† illustrates the synthesized crushed MAX powders with clearly laminar shapes. It is difficult to estimate the exact plate thickness of individual sheets, but groups of sheets are 40–200 nm in thickness. Fig. S1b† shows that the Ti3C2Tx MXene surface, after HF treatment, is typically delaminated from MXene with a thickness of 40–220 nm. In order to increase the interlayer spacing of the Ti3C2Tx MXene, the bonds between the Ti3C2Tx MXene layers were weakened by DMSO intercalation. The exfoliated Ti3C2Tx MXene obtained by DMSO treatment is shown in Fig. 1a, which features larger slots than before the DMSO exfoliation of the Ti3C2Tx MXene. As the single layer of Ti3C2Tx MXene flakes is 1 nm thick,37 as-obtained Ti3C2Tx MXene flakes by DMSO treatment are approximately 10–70 nm thick, corresponding to 10–70 layers multilayer. The FESEM image of the Ni-dMXNC shown in Fig. 1b demonstrates the increased dimensions (horizontal as well as vertical) of individual nanosheets and the growth of vertical NiO nanosheets between horizontally stacked modified Ti3C2Tx MXene layers, suggesting the successful addition of the NiO nanosheets. The flower-like NiO composed of several nanosheets is confirmed in Fig. S4a,† which shows hierarchical microspheres. The electrical properties of pure Ti3C2Tx MXene and Ni-dMXNC determined from using Hall-effect measurement system, as shown in Table S1 (ESI†). From the resistance measurements of Ti3C2Tx MXene and Ni-dMXNC, it is clearly indicated that the conductivity of Ni-dMXNC is superior to pure Ti3C2Tx MXene. With the combined features of the modified Ti3C2Tx MXene and NiO, the composite have the increased surface area and the active NiO covering, thus increasing electrode/electrolyte interfacial contact area, shortening diffusion paths for both electrons and ions, and improving conductivity; any of these may improve the electrochemical performance compared to those of pristine and modified Ti3C2Tx MXene. Fig. 1c demonstrates the typical XRD patterns of the MAX before and after HF treatment, showing a phase change from MAX to Ti3C2Tx MXene. The well-defined diffraction peaks observed at 2θ values of 9.2°, 19.2°, 34.0°, 36.7°, 39.0°, 41.8°, 48.5°, 52.4°, 56.6°, 60.2°, 65.6°, 70.5°, and 74.1° are indexed to the (002), (004), (100), (103), (104), (105), (107), (108), (109), (110), (1011), (118) and (1013) planes, respectively, of the MAX Ti3AlC2 (JCPDS 52-0875). After etching, almost all Al is removed from this structure; the (002) and (004) planes of the MAX phase are shifted to lower angles, indicating larger d spacings in MXene than in MAX.11 For the XRD pattern of MXene, it can be found that there are some peaks of TiO2 at ∼25°, 37° and 47° (Fig. 1c), indicating that MXene has been partially oxidized. The XRD pattern of Ni-dMXNC (Fig. 1d) shows the presence of anatase TiO2 peaks (01-071-1167), indicating that TiO2 derived from Ti3C2Tx MXene during the annealing and hydrothermal process.38 TiO2 is an outstanding electrode materials in energy storage due to its low potential, good cycle stability and fast lithium intercalation.39,40 So, the derived TiO2 hold great promise on improving the electrochemical performance of MXene-based electrode materials. New peaks at 2θ values of 37.1°, 43.2°, 62.9°, 75.2°, and 79.6° were assigned to the (111), (200), (220), (311), and (222) planes of NiO (JCPDS 01-078-0643).
To investigate the formation mechanism and the spatial distributions of corresponding elements of the Ni-dMXNC, elemental mappings were performed (Fig. 2). The elemental mapping displays the uniform coverage of Ni on the modified Ti3C2Tx MXene. In Fig. S2,† the energy dispersive X-ray spectroscopy (EDS) analyses of Ti3C2Tx MXene and Ni-dMXNC clearly reveal the corresponding elemental contents with an atomic ratio. The Ti3C2Tx MXene contains T, C, F, O elements with an atomic ratio of Ti
:
C
:
O
:
F = 27
:
15
:
11
:
10 (Fig. S2e†). The selected area EDS of Ni-dMXNC (Fig. S2d†) comprises Ni, O, C, and Ti. The corresponding elemental contents in Fig. S2f† reveal that the main constituents are Ti, C, Ni, and O with an atomic ratio of Ti
:
C
:
Ni
:
O = 34
:
14
:
10
:
34. Note that the C content lower than the stoichiometric of the Ti3C2 may be attributed to the production of carbon dioxide by the oxidization of carbon element along with the oxidization of other elements. The Ti
:
Ni atomic ratio of the as-obtained Ni-dMXNC is calculated at 3.4
:
1.
High-resolution XPS measurements were utilized to characterize the chemical composition and valence states of the elements in pure MXene (Fig. S3†) and Ni-dMXNC (Fig. 3). In the Ti 2p spectrum (Fig. S3a†), Ti 2p core level was fitted with two doublets (Ti 2p3/2–Ti 2p1/2) with a fixed area ratio equal to 2
:
1 and a doublet separation of 5.7 eV. The Ti 2p3/2 components were located at 455.0 eV and 456.2 eV, which corresponding to Ti–C and Ti–X bond, respectively.41,42 Ti 2p1/2 components were located at 460.8 eV and 462.7 eV corresponding to C–Ti–Ox and Ti–O, respectively.43 The C 1s (Fig. S3b†) peaks at 281.1 eV and 284.6 eV corresponding to Ti–C and C–C bond, respectively.41,44 The O 1s spectrum (Fig. S3c†) are fitted using 2 components located at 529.8 eV and 531.8 eV corresponding to O 1s in TiO2 and hydroxyl groups.45 The F 1s XPS (Fig. S3d†) shows a predominant peak at 863.7 eV, corresponding to Ti3C2F.
![]() | ||
| Fig. 3 (a) High-resolution XPS survey spectra. (b) Ti 2p, (c) C 1s, (d) Ni 2p, (e) O 1s, and (f) F 1s spectra of Ni-dMXNC. | ||
The high-resolution XPS spectra Ti 2p and C 1s of Ni-dMXNC were presented in Fig. 3b and c. Ti 2p core level was fitted with two doublets (Ti 2p3/2–Ti 2p1/2) with a fixed area ratio equal to 2
:
1 and a doublet separation of 5.7 eV. The Ti 2p3/2 peak located at 455.0 eV corresponds to Ti–C in the core. The 458.0 eV (Ti 2p3/2) and 463.7 eV (Ti 2p1/2) peaks are ascribed to Ti–O on the surface.46,47 The Ti–O is from the oxidation of MXene (TiO2). The C 1s (Fig. 3c) peaks at 281.0 eV, 284.6 eV, and 286.0 eV are assigned to the characteristic bonds of C–Ti, C–C, and C–O, respectively.44 The Ni 2p spectrum, as shown in Fig. 3d, presents two obvious satellites (indicated as “Sat”) and Ni 2p3/2 and Ni 2p1/2 peaks at 855.9 eV and 873.6 eV, both supporting the presence of Ni2+. We observe two O environments of NiO in the O 1s XPS (Fig. 3e): the O 1s peak located at 529.3 eV is ascribed to O–Ni and that at 531.1 eV to O–H, confirming the presence of several hydroxyl groups (Ti–OH) to form the Ti3C2(OH)2 covering the Ti3C2Tx MXene surface.6 The F 1s XPS (Fig. 3f) shows a predominant peak at 863.7 eV, corresponding to Ti3C2F. These results clearly show the abundance of functional groups and the availability of electroactive sites like –OH, –F, Ti4+, and Ni2+ in Ni-dMXNC, which are conducive to the high rate capacity and long-range cycling stability of supercapacitors.
The typical morphological and structural characterizations were further investigated by TEM (Fig. 4 and S4†). Fig. S4a (ESI†) shows the NiO nanosheets in a hierarchical porous sphere shape. In the high-resolution TEM (HRTEM) image (Fig. S4b, ESI†), a 0.207 nm lattice fringe spacing for NiO (200) is evidenced; in the corresponding selected-area electron diffraction (SAED) pattern (Fig. S4c, ESI†), polycrystallinity is verified. The exfoliated Ti3C2Tx MXene, as seen in Fig. 4a–c, presents a 0.352 nm lattice fringe spacing corresponding to anatase TiO2 (101) and the corresponding SAED patterns shows the hexagonal symmetry of the flakes and single-crystal nature of the modified Ti3C2Tx MXene,48–50 suggesting that the TiO2 particles are nucleated on the external or interior Ti3C2Tx MXene layers, which agrees well with the Ti3C2Tx MXene XRD analysis. Fig. 4d–f provides structural information on the Ni-dMXNC. The low-magnification TEM image shows that NiO nanosheets grow on the Ti3C2Tx MXene. The SAED pattern of the corresponding HRTEM image of the Ni-dMXNC is shown in Fig. 4f and corroborates the polycrystalline nature of the modified MXene. The TEM results agree well with the above XRD and XPS measurements.
To further investigate the surface properties of the Ni-dMXNC, Brunauer–Emmett–Teller (BET) results are presented in Fig. S5 (ESI†) A typical type-IV isothermal and an H3-type hysteresis loop in the relative pressure (P/Po) range of 0.5–1.0 are obtained. These indicate the formation of slit-like pores in the Ni-dMXNC mesoporous structure. The presence of two peaks at 3 and 20 nm in the pore-size distribution plot indicates excess mesoscale pores.51,52 The specific surface areas, pore size, and total pore volumes of the Ti3C2Tx MXene and Ni-dMXNC are, respectively, 10.0 m2 g−1 and 77.5 m2 g−1, 24.1 nm and 21.1 nm, and 0.02 cm3 g−1 and 0.20 cm3 g−1 (Table 1), suggesting the superiority of the latter relative to the former. The high surface area of the Ni-dMXNC could enhance its electrochemical properties, as the pore channels facilitate rapid electrolyte transportation to the surface of the active materials. In addition, the defects formed during the phase change could provide more active sites for redox reactions.53
| Sample | Pore size (nm) | SBET (m2 g−1) | Vpores (cm3 g−1) |
|---|---|---|---|
| Ti3C2Tx | 24.1 | 10.0 | 0.02 |
| Ni-dMXNC | 21.1 | 77.5 | 0.20 |
EIS analysis is routinely used to evaluate the ion transportability across the electrolyte/electrode interface in supercapacitor applications. The EIS analyses of the Ti3C2Tx MXene and Ni-dMXNC electrodes were obtained from 100 kHz to 0.01 Hz using a three-electrode system (Fig. 5e and f). The impedance spectra, in the form of Nyquist plots, demonstrate sharp semicircles intersecting the real axis in the high-frequency regions and nearly vertical lines in the low-frequency regions. The high-frequency intercept (100 kHz) represent the equivalent series resistance (Rs) across the electrode/electrolyte, which reflects the contribution from the electronic, electrolyte, contact, and internal resistances of the active materials.56 The semicircle, formed by double-layer capacity (Cdl) and charge-transfer resistance (Rct), confirms the charge-transfer process across the electrode/electrolyte interface. At low frequency, the sloped curve, relating to the electrolyte diffusion in the active materials, reflects the Warburg resistance (Zw).57 The Rs, Rct, and Zw values of the Ti3C2Tx MXene electrode are 1.057 Ω, 46.780 Ω, and 5.727 Ω, respectively, while for the Ni-dMXNC electrode these are reduced to 0.960 Ω, 0.383 Ω, and 1.653 Ω. These lower Rs and Rct values of the Ni-dMXNC electrode compared to those of the Ti3C2Tx MXene electrode indicate the higher conductivity of the former. The decreased Zw value may be from the high surface area of the Ni-dMXNC electrode, which facilitates fast electrolyte ion diffusion to the active sites and surface of the Ni-dMXNC. The Ni-dMXNC electrode reveals a higher Cdl value of 3.375 F, compared to 0.066 F, than the Ti3C2Tx MXene electrode does, indicating that the presence of the 3D porous NiO nanosheets contributes to the specific capacity of the Ni-dMXNC electrode.
In the CV spectra obtained at a scan rate of 10 mV s−1 of the Ti3C2Tx MXene and Ni-dMXNC electrodes (Fig. 6a), a pair of redox peaks with an anodic peak at 0.55 V and a cathodic peak at 0.39 V is observed for the Ti3C2Tx MXene electrode, whereas a pair of redox peaks with an anodic peak at 0.51 V and cathodic peak at 0.30 V occurs for the Ni-dMXNC electrode, indicating the presence of strong faradaic behaviour in both electrodes. Moreover, the average area under the Ni-dMXNC electrode CV curve is higher than that of the Ti3C2Tx MXene electrode, suggesting that the Ni-dMXNC shows higher electrochemical performance than the MXene. In this case, the Ni foam acting as a current collector in the electrode produced a flat line in the CV curve, indicating that the capacity of the Ni foam is negligible.58,59 In the diffusion-controlled electrochemical redox reaction, the peak current ip is calculated according to the Randles–Sevcik equation:60
![]() | (7) |
is the reactant concentration, and ν is the scan rate. The relationships between the positive peak current (Ip,c) and the scan rate (ν) of the Ti3C2Tx MXene and Ni-dMXNC composite electrodes are shown in Fig. 6b. Ip,c increases linearly with ν1/2, confirming that the faradaic nature of both electrodes is limited by the diffusion of OH− to the active sites. The diffusion coefficients of the Ni-dMXNC composite electrode (DNi-dMXNC) exhibiting higher diffusion coefficients compare with Ti3C2Tx MXene (DTi3C2Tx). This result was further confirmed by the GCD measurements of Ti3C2Tx MXene and Ni-dMXNC electrodes at the current density of 1 A g−1 (Fig. 6c). The QD values of Ti3C2Tx MXene and Ni-dMXNC electrodes (Fig. 6d) were calculated from the GCD curves at current densities of 1, 2, 3, 4, 5, 8, and 10 A g−1. The QD values of the Ti3C2Tx and Ni-dMXNC electrodes are 8.2, 7.3, 6.6, 5.8, 5.6, 4.1 and 4.4 mA h g−1, and 60.7, 56.2, 52.4, 49.5, 47.0, 39.7 and 35.6 mA h g−1, respectively. The capacity of the Ni-dMXNC electrode with increasing current density from 1 to 10 A g−1 was retained to 58.6% based on the initial capacity value, which is higher than the 53.7% of the capacity-reduced ratio of the Ti3C2Tx MXene electrode under the same current conditions. The specific capacity to reach 60.7 mA h g−1 at a current density of 1 A g−1, corresponding to a volumetric specific capacity of 92.0 mA h cm−3, is significantly superior to that measured on a Ti3C2Tx MXene-based electrode (Table S2, ESI†).20,61,62 Compared to the Ti3C2Tx MXene electrode, the Ni-dMXNC electrode demonstrates considerably higher capacity and a better rate capability than the Ti3C2Tx MXene electrode. This could be because of: (i) the synergistic effect generated in Ni-dMXNC by the two morphologies and porosities, as well as by the higher surface area. The presence of porous NiO between the modified Ti3C2Tx MXene sheets could yield minimal density, relatively high out-of-plane compression properties, and good in-plane elastic properties, increasing the number of redox reactions.63 This dual morphology of MXene and NiO is advantageous for electrolyte ion diffusion into the electrode material, while showing excellent chemical stability as confirmed by the cycling test. (ii) The functional groups on the surface of Ti3C2Tx MXene are responsible for the enhanced faradaic capacity in the Ni-dMXNC electrode. (iii) The annealing process, which might have separated the graphite and TiO2 to a formation of carbon-supported TiO2 hybrids results in an enhanced conductivity and specific surface area, and increased NiO crystallization, was responsible for the decreased internal and faradaic Rct values, as demonstrated in the EIS discussion. The cyclic performances of the Ti3C2Tx MXene and Ni-dMXNC electrodes were evaluated for 5000 charge/discharge testing cycles at a current density of 5 A g−1 (Fig. 6e). The Ti3C2Tx MXene electrode exhibited excellent cycling performance with only 3.6% degradation after 5000 cycles at a current density of 5 A g−1, but was very low capacity. For the Ni-dMXNC electrode, the capacity (QD) was rapidly increased from 47.0 to 48.5 mA h g−1 to first 100 cycles due to the initial activation of the electrode, slowly dropped to 35.3 mA h g−1 to 2500 cycles, and stabilized to 33.1 mA h g−1 after 4400 cycles. The capacity retention of the Ni-dMXNC electrode after 5000 cycles exhibited a moderate improvement of about 70.4%, attributed to the decorated NiO on the Ti3C2Tx MXene (about 64.3% retention of a pure NiO electrode after 5000 cycles as shown in Fig. S7†). For purpose of improving the capacitive properties of the positive electrode in a hybrid asymmetric cell, it would be highly desirable to boost the performance of the negative electrode. With the purpose of the capacity balance of a positive electrode and a negative electrode, it is necessary to be a suitable mass ratio of the positive electrode
:
negative electrode. The GCD curves of asymmetric cells with the potential change of each individual electrode in situ were monitored by an auxiliary channel and a reference electrode (mercury/mercury oxide) (Fig. S8†). The applied current for each electrode was kept at 1 mA. The positive electrode (Ni-dMXNC) was swept between 0 to 0.8 V, while the negative electrode (Ti3C2Tx MXene) was scanned at 0 to −1 V. When a mass ratio of the positive and negative electrodes was 1
:
4.39, they exhibited similar capacity.
In order to evaluate the applicability of Ni-dMXNC electrodes in practical supercapacitors, we fabricated an ASC with a Ni-dMXNC positive electrode, Ti3C2Tx negative electrode, and electrolyte of 1 M KOH (denoted as Ni-dMXNC//Ti3C2Tx), as illustrated in Fig. 7e. To achieve the maximum full-cell capacity, the charge balance followed the relation q+ = q−, where q+ and q− represent the positive and negative electrode charges, respectively. The charge storage was on q = C × ΔE × m.64 From the charge balance, the ASC device should have a positive-negative electrode mass ratio of 0.23. The electrochemical properties of the Ni-dMXNC//Ti3C2Tx ASC were tested in a two-electrode system. Fig. 7a presents the CV curves obtained from the fabricated Ni-dMXNC//Ti3C2Tx ASC device at different scan rates in the 0–1.8 V potential window. The faradaic capacity contribution causes a pair of evident redox peaks to appear in the curves. The charge/discharge curves obtained at various current densities are shown in Fig. 7b and suggest non-linearity because of the contributions to the redox reaction by the NiO and modified Ti3C2Tx MXene, consistent with the CV curves. The QD (Fig. 7c) of the Ni-dMXNC//Ti3C2Tx ASC device was 4.7, 4.4, 3.9, 3.8, 3.5, 3.3, 2.3, 1.7 and 1.2 mA h g−1 at current densities of 0.1, 0.2, 0.4, 0.6, 0.8, 1.0, 1.6, 2.0 and 3.0 A g−1, respectively (based on the total mass of each electrode in a device). To further investigate the cycling stability of the ASC device, the cycling performances within 0–1.8 V at a current density of 1 A g−1 were observed over 5000 cycles. In first 800 cycles, the QD tended to decreases rapidly as NiO may be activated by KOH electrolyte (Fig. 7d). In subsequent cycles, the capacity of the ASC device dropped smoothly and exhibited a 72.1% retention rate after 5000 cycles. In a Ragone plot shown in Fig. 7f, an ASC device consisting of Ni-dMXNC as a positive electrode and Ti3C2Tx as a negative electrode delivered an energy density of 1.04 × 10−2 W h cm−3 at a power density of 0.22 W cm−3. When the power density was 5.88 W cm−3, the energy density was 2.29 × 10−3 W h cm−3. The energy density value calculated based on the volume of active electrodes is much higher than most reported Li thin film battery,65 metal oxide based SCs,31 commercial SC,66 carbon-based micro-SCs.65,67 Moreover, it's comparable to the areal energy/power density of NiCo2S4//CNF hybrid device and clay-like Ti3C2 MXene MSCs.68,69 To demonstrate the application potential of the Ni-dMXNC//Ti3C2Tx ASC device, we connected two ASC coin cells in series to drive a red light-emitting diode for 12 min (Fig. 7f (inset)). The long-term ON performance is attributed to the Ni-dMXNC structure and the unique 3D morphology, which could provide numerous channels to enhance the ion transport kinetics across the electrode–electrolyte interface. Ni-dMXNC could also permit electrolyte ions to intercalate/deintercalate without structural distortion, as demonstrated by the good cycling stability. These results show that Ni-dMXNC may be a promising positive electrode material for ASCs in the future.
![]() | ||
| Fig. 7 (a) CV curves of Ni-dMXNC//Ti3C2Tx asymmetric supercapacitor at different scan rates; (b) GCD curves of Ni-dMXNC//Ti3C2Tx asymmetric supercapacitor; (c) capacity retention of Ni-dMXNC//Ti3C2Tx asymmetric supercapacitor at different current densities; (d) cycling performance of the Ni-dMXNC//Ti3C2Tx asymmetric supercapacitor at a current density of 1 A g−1; (e) schematic of the Ni-dMXNC//Ti3C2Tx asymmetric supercapacitor configuration with each SEM image; (f) Ragone plot of Ni-dMXNC//Ti3C2Tx ASCs. The comparison of energy and power density of Ni-dMXNC//Ti3C2Tx ASCs, Li thin film battery,65 metal oxide,31 commercial SC,66 and carbon micro-SCs,65,67 demonstrating that Ni-dMXNC//Ti3C2Tx ASCs exhibit exceptional electrochemical energy storage with simultaneous high energy density and power density. | ||
This work demonstrates that the as-obtained Ni-dMXNC nanostructures are promising electrode materials for the further development of high-performance energy-storage devices.
Footnote |
| † Electronic supplementary information (ESI) available: FESEM images of Ti3AlC2 MAX phase, Ti3C2Tx MXene and NiO, EDX of Ni-dMXNC, TEM images of NiO nanosheets, adsorption–desorption isotherms of Ti3C2Tx MXene and Ni-dMXNC, CV curves of Ti3C2Tx MXene and Ni-dMXNC, Fig. S1–S8. Resistivity of the Ti3C2Tx MXene and Ni-dMXNC materials, Table S1. Comparison of maximum gravimetric capacity and volumetric capacity of the reported MXene-based materials and the present work, Table S2. See DOI: 10.1039/c6ra27880a |
| This journal is © The Royal Society of Chemistry 2017 |