Open Access Article
This Open Access Article is licensed under a Creative Commons Attribution-Non Commercial 3.0 Unported Licence

Tunable multilayer assemblies of nanofibrous composite mats as permeable protective materials against chemical warfare agents

S.-Y. Ryua, J. W. Chung*b and S.-Y. Kwak*a
aDepartment of Materials Science and Engineering, Seoul National University, 1 Gwanak-ro, Gwanak-gu, Seoul 08826, Korea. E-mail: sykwak@snu.ac.kr; Fax: +82-2-885-9671; Tel: +82-2-880-8365
bDepartment of Organic Materials and Fibre Engineering, Soongsil University, 369 Sangdo-ro, Dongjak-gu, Seoul 06978, Korea. E-mail: jwchung@ssu.ac.kr; Fax: +82-2-817-8346; Tel: +82-2-828-7047

Received 25th September 2016 , Accepted 23rd December 2016

First published on 20th January 2017


Abstract

Lightweight nanofibrous assemblies with high protection ability against chemical warfare agents (CWAs) were developed using laminated outer and inner layers based on nanofibre composites. The outer layer was composed of a meta-aramid nanofibre and CWA adsorbents (MgO and POM), and possessed high mechanical strength and an amphiphobic surface capable of repelling liquid CWAs. The inner layer, consisted of a polyamide 66 nanofibre and CWA adsorbents, exhibited low permeability to gas CWAs and high permeability to water vapor. These outer and inner layers were prepared by simultaneous electrospinning and electrospraying processes. By controlling the stacking of the inner and outer layers, the characteristics of their assemblies, such as thickness, weight density, and cool/warm feeling, were improved. In addition, the assemblies resisted the invasion of CWAs, while still maintaining considerable water vapor transmission to allow evaporative cooling of the wearer. Based on these results, assemblies composed of nanofibrous composite can be used as in garments that protect wearers from various contaminants such as organic pollutants and harmful particulates, as well as from CWAs.


Introduction

Chemical warfare agents (CWAs) have been used in tactical warfare as incendiary mixtures, smoke, and irritating, burning, poisonous, or asphyxiating gases.1 CWAs have been classified according to their target organs or tissues as nerve, vesicant, choking, blood and vomiting agents, as well as incapacitants and lacrimators.2 Many CWAs are dermally active; therefore, a number of studies on materials that provide protection against CWAs have been performed.3–5 There are various types of defense equipment available to protect the body from CWAs, including detectors, respirators, protective clothing, decontaminants and medical counter measures.6 Protective clothing can be classified into impermeable and permeable categories. Impermeable protective clothing offers powerful protection against CWAs, but is unfit for long-term wear because it is cumbersome and uncomfortable. In contrast, permeable protective clothing is composed of outer and inner layers to make it breathable. The outer layer repels the liquid CWA that is trying to penetrate the protective clothing. The inner layer consists of nonwoven fabric or porous foam impregnated with an adsorbent, such as activated carbon, to chemisorb any gas CWA that enters through the outer layer.

The activated carbon materials used in permeable protective clothing is impregnated with nanoparticles composed of silver, tin, zinc or molybdenum, along with triethylenediamine. A popular example of a permeable protective garment containing activated carbon materials is the joint service lightweight integrated suit technology (JSLIST) overgarment, which has been used by the US Army.7 Permeable protective clothing like the JSLIST suit offers complete protection against CWAs, but it has associated disadvantages such as moisture retention and heavy weight (2.63 kg per overgarment), resulting in discomfort. These disadvantages prevent users from wearing JSLIST suits for more than 6–8 h at a time. Therefore, there is a need to develop a more comfortable clothing that is light, with high moisture permeability, but that still protects the wearer from CWAs.

A number of protective materials with higher adsorption capacity, lighter weight and greater comfort than their predecessors have been designed. Catalysts and adsorbents with detoxification activity such as MgO,8,9 MnO2,10 ZnO,11,12 TiO2,13 ZnTiO3,14 M/TiO2/SiO2 (M = Fe, Mn, and V),15 WO3/titanate,16 N-doped TiO2,17 Au/TiO2,18 and polyoxometalate (POM)19 have been actively investigated as the fillers incorporated in such permeable protective clothing. Among these fillers, MgO has been widely studied as an effective catalyst against the sarin, nerve agent, because it is highly active and can readily decompose this nerve agent.20 MgO can physisorb CWAs on its surface through the formation of hydrogen-bonding, ion–dipole and dipole–dipole interactions.21 In addition, POM has been considered as a reactive and recoverable catalyst for the decontamination of vesicant agents such as sulfur mustard (HD).22,23

The disadvantages of existing permeable protective clothing can be overcome by replacement with lightweight materials composed of structures such as nanofibres. Nanofibres, like all other electrospun nanostructures,24–26 show improved properties compared with those of conventional fibres because of their small dimensions and unique features, such as high surface-to-volume ratio, small fibre-to-fibre distance, high porosity, large specific surface area, small pore size, and high controllability. These unique characteristics, plus the functionalities of the materials themselves, impart nanofibres with a number of novel properties that are attractive for advanced applications. Nanofibres have been used in protective clothing for CWAs, as well as for biological warfare agents. Various methods to modify nanofibre surfaces to enhance their protection and decontamination capabilities have been developed based on chemical surface modification and attachment of reactive groups on the nanofibre surface, and especially functionalized nanofibres for protection from chemical warfare simulants based on hydrolysis have been developed and evaluated.27 In addition, catalysts, such as MgO and POM, were incorporated into nanofibres, and the resulting nanofibre-bound catalysts decontaminated CWAs.8,28

Herein, we demonstrate a potential application of nanofibrous composite materials impregnated with MgO and POM adsorbents as the inner and outer layers, respectively, of permeable materials that are protective against CWAs. The inner and outer layers of the composite nanofibre mats are stacked on one another to assemble protective clothing materials. The outer layer consists of both meta-aramid nanofibres and the absorbents and has an amphiphobic nature, so the liquid CWA simulants bounce off it. The inner layer is composed of Nylon 66 nanofibres with MgO and POM as absorbents, and plays a role in protection by adsorbing gas CWA simulants. The assembly of these two layers improved the thickness, weight, water vapor transmittance, cool/warm feeling and protection against CWA simulants compared with the corresponding properties of existing permeable protective clothing materials. In particular, the thickness and weight density of the material depended on the number of stacked layers. Lightweight assemblies with high protection against CWAs were developed. These assemblies provide good resistance to the penetration of gaseous CWAs, while still allowing water vapor transmission to promote evaporation cooling of the wearer. The assembly of multiple layers developed here reveals a new approach to improve the performance of permeable protective materials, and will aid the design and optimization of permeable protective clothing.

Experimental

Materials

Commercial MgO (light and heavy grade), POM (ammonium (para)tungstate hydrate, (NH4)10(H2W12O42)·4H2O, and ammonium phosphomolybdate hydrate, (NH4)3PMo12O40·nH2O) as absorbents of the chemical warfare agent (CWA) simulants were purchased from various manufacturers, as listed in Table 1. All samples were stored under ambient conditions before adsorption testing. 2-Chloroethyl ethyl sulfide (2-CEES; 98% GC purity) and dimethyl methylphosphonate (DMMP, 97% GC purity) were purchased from Sigma-Aldrich (USA) as CWA simulants of mustard gas and sarin, respectively. All materials were used as received without further purification. Poly(meta-phenylene isophthalamide) (meta-aramid, Nomex, DuPont, USA), N,N-dimethylacetamide (DMAc, anhydrous, 99.8%, Sigma-Aldrich, USA), lithium chloride (LiCl, ACS reagent, ≥99%, Sigma-Aldrich, USA), Unidyne TG-5601 (water-based emulsion; 20–30% fluoroalkyl acrylate copolymer, 5% poly(oxyethylene) alkyl (C12–14) ether, 1–10% tripropylene glycol, 55–65% water and 5% other materials; weak cation; as water and oil repellent, Daikin, Japan) were used as received without further purification. Poly(hexamethylene adipamide) (polyamide 66, Nylon 66, Sigma-Aldrich, USA), formic acid (≥95%, Sigma-Aldrich, USA) and benzyltrimethylammonium chloride (BTMAC, ≥99.0%, Tokyo Chemical Industry, Japan) were used as received without further purification.
Table 1 Adsorptivity of chemical warfare agent simulants 2-CEES and DMMP by MgO and POM particles
Manufacturer Sigma Aldrich Daejung Junsei Wako
MgO −325 mesh <50 nm Light Heavy Light Heavy Light
2-CEES adsorptivity (μg g−1, (%)) 0.22, (28.8) 0.18, (23.1) 0.30, (38.2) 0.32, (41.7) 0.24, (31.2) 0.13, (17.5) 0.26, (33.3)
DMMP adsorptivity, (μg g−1, (%)) 0.93, (78.3) 0.82, (68.5) 0.64, (53.4) 0.61, (51.2) 0.78, (65.6) 0.47, (39.3) 0.54, (45.6)
Suitable for electrospraying Yes Yes Yes Yes Yes Yes Yes

POM (NH4)10(H2W12O42)·4H2O (NH4)3PMo12O40·nH2O
Manufacturer Sigma Aldrich Daejung Kanto
2-CEES adsorptivity (μg g−1, (%)) 0.61, (79.8) 0.57, (74.0) 0.72, (93.7)
DMMP adsorptivity (μg g−1, (%)) 0.72, (60.7) 0.79, (66.4) 0.87, (73.0)
Suitable for electrospraying No Yes Yes


Adsorptivity of CWA simulants on MgO and POM particles

The adsorption of the simulants on the adsorbents (MgO and POM) was measured according to ASTM D5160-95.29 To produce the gas of CWA simulants, 2-CEES (1 mL; vapor pressure of <3.4 mmHg at 25 °C and volatility of 16[thin space (1/6-em)]570 mg m−3 of at 20 °C) was added to ethanol (199 mL), and of DMMP (10 mL; vapor pressure of 1 mmHg at 25 °C and volatility of 347 mg m−3 at 20 °C) was added to ethanol (190 mL). Then 200 mL of each CWA simulant/ethanol solution was put in a bubbler and placed in a water bath at a temperature of 74 ± 1 °C. This action was performed to ensure that the simulant gas was formed effectively in the tubing and maintained at the same temperature. The adsorbent (500 mg) was fixed in a cylindrical sample chamber with 10 mm radius, and the adsorption temperature was controlled at 35 °C. Simulant solution (1% v/v in ethanol) was purged with dry N2 gas, so that the adsorbate vapor was generated continuously, and the vapor was passed through the absorbent at a flow rate of 50 cm3 for 40 min. The expelled gas was trapped in a Tenax-TA tube, and desorption of the simulants trapped in the Tenax-TA tube was conducted using thermal desorption gas chromatograph mass spectrometry (TDS-GC-MS, GC: 6890N, Agilent; MSD: 5975, Agilent; TDS: TDS2, Gerstel). The types of MgO and POM showing the best performance MgO and POM were finally selected as adsorbents. These adsorbents were doped in polymeric nanofibres to form the inner and outer layers of protective materials using the simultaneous electrospinning and electrospraying (SEE) process.

Nanofibrous outer layer for repellent protection against CWA simulants

The composite nanofibre for the outer layer consisting of meta-aramid nanofibre (mANF) and selected absorbent (MgO or POM) was prepared using the SEE process30 (Fig. S1). The SEE apparatus was constructed with a rotating drum collector, two positive DC voltage supplies, one negative DC voltage supply, and two syringe pumps composed of housings with syringe retainers. These syringe pumps were placed on opposite sides to the collector. To prepare the electrospinning solution of mANF, Nomex fibre (8 g) was dissolved in DMAc solution (50 mL) containing LiCl (1.6 g) as a salt (1[thin space (1/6-em)]:[thin space (1/6-em)]5 weight ratio of LiCl/Nomex) at 50 °C for 24 h in an oven shaker (BF-30SI, BioFree, Korea). Pristine mANF was prepared by electrospinning as follows. A syringe with a stainless-steel needle with an internal diameter of 0.33 mm was filled with the electrospinning solution, which was then ejected at a flow rate of 0.15 mL h−1 for 68 h. The needle tip of the syringe was directly charged at 20–25 kV. The syringe was positioned horizontally with a tip-to-collector distance of 15 cm from a drum collector covered with Al foil rotating at 100 rpm. The collector was charged at −5 kV. The electrospinning process was conducted at 23 ± 1 °C and 45 ± 5 RH%. To introduce the adsorbents on the surface of mANF, MgO or POM (1 g) was dispersed in methanol (100 mL) using a horn-type ultrasonicator (VCX-750, Sonics & Materials, CT, USA) for 30 min. Each dispersion was electrosprayed using a stainless-steel spinneret with an internal diameter of 0.51 mm, applied voltage at the spinneret of 12 kV, tip-to-collector distance of 10 cm, and solution flow rate of 1.5 mL h−1 for 68 h. Using this SEE process, pristine MgO/mANF and POM/mANF samples with a thickness of 75 μm were prepared.

The as-prepared MgO/mANF and POM/mANF samples were fixed in stainless-steel frames for post-treatment. The samples were soaked in deionized water and gently shaken for 1 h to remove the LiCl salt and any unbound adsorbents from the nanofibres. The samples were heat-treated in air at 300 °C (above the glass transition temperature of a neat Nomex nanofibre, see Fig. S2) for 10 min in a processing oven (UF 110, Memmert, Germany) to enhance their chemical stability and mechanical properties. To generate amphiphobic surfaces, the heat-treated samples were treated with Unidyne (Daikin, Osaka, Japan), which is a fluorinated water and oil repellent. The samples were immersed in Unidyne (200 mL) for 10 min, and then stabilized for 10 min in air. The samples were transferred into the processing oven and heat treated at 180 °C for 3 min to give composite nanofibre mats with amphiphobic surfaces (denoted [O]MgO/mANF and [O]POM/mANF) for use as outer layers.

The surface morphology of [O]MgO/mANF and [O]POM/mANF was observed by field-emission scanning electron microscopy (FE-SEM, JSM-6335F; JEOL). The adsorbent content and thermal behavior of the composites was observed by simultaneous differential thermal analysis/thermal gravimetric analysis (DTA/TGA; SDT 2960; TA Instruments) using a heating rate of 10 °C min−1, temperature range of 40–700 °C, and N2 atmosphere. The repellency of the CWA simulants by each composite was determined by measurement of their static water contact angle (WCA) and oil contact angle (OCA). WCAs and OCAs were determined by contact angle measurements (Theta Lite; Attension; KSV Instruments) with a manually controlled Hamilton syringe. Apparent contact angles of water and simulant drops were measured in air at 25 ± 1 °C. A droplet with a volume of 3.0 ± 0.2 μL was formed on the surface of each nanofibre mat and droplet size was observed. Average WCAs and OCAs for results obtained at five different positions on each sample are reported, with standard deviations of ±2°.

Nanofibrous inner layer for adsorptive protection against CWA simulants

The composite nanofibres for the inner layer consisting of polyamide 66 nanofibres (PANF) and the selected adsorbents (MgO or POM) were also prepared by the SEE process. To electrospin PANF, first polyamide 66 pellets (5.4 g) were dissolved in of formic acid solution (36 mL) containing BTMAC (0.54 g) as a salt and gently shaken for 24 h at room temperature until the solution was transparent. The solution was electrospun using a stainless-steel spinneret with an internal diameter of 0.33 mm, applied voltages of 18–20 kV at the spinneret and −5 kV at the collector, a tip-to-collector distance of 9 cm, collector rotation speed of 100 rpm, and solution flow rate of 1.0 mL h−1 for 10 h at 22 ± 1 °C and 50 ± 5% RH. To introduce the adsorbents on the surface of PANF, absorbent (1 g) was dispersed in methanol (100 mL) using a horn-type ultrasonicator (VCX-750, Sonics & Materials, CT, USA) for 30 min. The dispersion was electrosprayed using a stainless-steel spinneret with an internal diameter of 0.51 mm, applied voltage of 12 kV at the spinneret, tip-to-collector distance of 10 cm, and solution flow rate of 10.0 mL h−1 for 10 h. The as-prepared samples were annealed at 80 °C for 30 min in a processing oven (UF 110, Memmert, Germany) to adhere the adsorbents on the surface of the nanofibres. The samples were washed four times with deionized water/methanol solution to remove the salt and any unbound absorbents from the nanofibres. Washed samples were dried at room temperature for 1 day in air and a vacuum oven, and stored in a vacuum desiccator. This process gave composite nanofibre mats (denoted [I]MgO/PANF and [I]POM/PANF) with a thickness of 91 μm for use as inner layers to protect against gas CWAs.

The morphology of the composite nanofibre mats was evaluated by FE-SEM (JSM-6335F; JEOL). The adsorbent content of the composites was determined by thermogravimetric analysis (TGA; Q5000 IR, TA Instruments) using a heating rate of 10 °C min−1, temperature range of 40–600 °C, and N2 atmosphere. The mechanical properties of the nanofibre mats were measured with a universal testing machine (UTM, Model 5567; INSTRON). Specimens with a width of 3.00 mm and thickness of 0.10–0.20 mm were prepared according to ASTM D638 Type V. The flow pore diameter and distribution of the nanofibre mats were measured with a capillary flow porometer (CFP-1500AEL; Porous Material Inc., USA) using SilWick silicone fluid (Porous Materials Inc.) with a surface tension of 19.1 dynes cm−1 as the wetting agent for porometry measurements. Air (0–100 psi) was used as a working gas. The air permeability of the nanofibre mats was measured according to the ASTM D737 standard. The water vapor transmission rate (WVTR) of the nanofibre mats was evaluated using the ASTM E96 standard. The permeation of gas CWA simulants (2-CEES and DMMP) through the nanofibre mats was determined by direct contact and dynamic diffusion permeation experiments according to a modified ASTM F739 standard, as illustrated in Fig. S3. In the case of a direct contact experiment, N2 gas with a flow rate of 50 cm3 min−1 (50 mL min−1), which was regulated using a flow meter (MKP, MPR-3000 s), delivered gas CWA simulants to the PANF mats for 20 min. Then, the simulant gas (1000 cm3) was passed through the mats (area of 4.9 cm2 and thickness of 180 μm) and collected by the Tenax-TA tube. The captured gas was evaluated by thermal desorption gas chromatography-mass spectrometry (TD-GC-MS). The equipment required for TD-GC-MS was connected to the setup with Teflon and Tygon tubing. In the case of dynamic diffusion experiments, the simulant gas was passed over the upper surface of a nanofibre mat along an upstream line at a flow rate of 50 cm3. At the same time, N2 carrier gas at a flow rate of 50 cm3 travelled along a downstream line, delivering the simulant gas that passed through the nanofibre mat (area of 25.5 cm2 and thickness of 180 μm) to the Tenax-TA tube for 40 min. The captured gas (2000 cm3) was evaluated by TD-GC-MS.

Assembly of the outer and inner layers to form nanofibrous protective materials against CWA simulants

To fabricate the nanofibrous protective materials, assemblies of the outer and inner layers were prepared by a spray- and heat-bonding process (Fig. S4). Multiple layers were sequentially positioned on top of one another. First, the spray glue was spread on an inner layer through a mesh to minimize the loss of available active area on its surface. Another inner layer was then placed above the adhesive surface of the bottom layer. This procedure was repeated one to seven times. The outer layers were positioned on the inner layers perpendicular to the direction of nanofibre alignment (rotated 90° between adjacent layers). Finally, assemblies composed of two outer layers and two to eight inner layers were obtained by heat-pressing at 80 °C under 500 psi for 10 min using a hydraulic press (Carver, model 2702, USA).

To examine the physical characteristics of the assemblies, various characterization techniques, such as air permeability, WVTR, and maximum heat transfer rate (qmax), were investigated using the standard methods ASTM D737, ASTM E96, and KES-F7 Thermo LaboII, respectively. The cool/warm feeling of the assembly was examined by measuring qmax (ref. 31) using a Thermo Labo II (KES-F7, KATO Tech Co., Japan), the main components of which were a temperature-detecting box (T-Box) and bottom-temperature box (BT-Box). The assembly, which was maintained at 20 °C, was positioned between the T-Box and BT-Box, which were heated to 32 °C to simulate human skin. Then, qmax was quickly measured for 0.2 s from the moment of contact. The reported results are the average of five experiments. The permeation of gas CWA simulants (2-CEES and DMMP) through each assembly was determined by permeation experiments according to the TOP 8-2-501 standard, as outlined in Fig. S5. The TOP 8-2-501 test method is based on the static diffusion procedure described in the U.S. Army Test and Evaluations Command Test Operations Procedure.32 The permeation test cell was composed of a cap and a base. A circular sample was positioned on the base containing a central well with a 5.7 cm diameter and inlet and outlet ports connected to Tygon tubing. The liquid simulant (2-CEES or DMMP) was dropped onto the surface of the sample at a fixed ratio of 10 g m−2 based on sample area. A cap covered the top of the sample and simulant to limit escape of the evaporated gas simulant. The liquid simulant on the sample evaporated into the space covered by the cap, and then the gas simulant crossed through the sample. Input N2 gas that delivered gas simulant (2000 cm3) to the Tenax-TA tube was regulated using a flow meter (MKP, MPR-3000s) with a flow rate of 200 cm3. The captured gas was evaluated by TD-GC-MS.

Results and discussion

Adsorptivity of CWA simulants on MgO and POM particles

To select suitable adsorbents to incorporate into composite nanofibres to form nanofibrous inner layers of protective materials against gas CWAs, we investigated the absorptivity of seven types of commercial MgO (light and heavy grade) and three types of POM for 2-CEES and DMMP according to the ASTM D5160-95 standard. As shown in Table 1, MgO candidates showed low absorptivity of 2-CEES (<0.32 μg g−1) at room temperature, but moderate absorptivity of DMMP (0.47–0.93 μg g−1). In contrast, POM species ammonium (para)tungstate hydrate and ammonium phosphomolybdate hydrate showed relatively higher absorptivity of 2-CEES (0.57–0.72 μg g−1) and moderate absorptivity of DMMP (0.72–0.87 μg g−1) compared with that of MgO samples. In addition, we checked the processability of the MgO and POM particles for electrospraying. Only ammonium (para)tungstate hydrate did not disperse in solvents such as methanol for electrospraying. Other candidates dispersed well in methanol, so they could be incorporated into composite nanofibres by electrospraying. Considering both the adsorption efficiency of CWA simulants and electrospraying ability of the various MgO and POM candidates, we selected a fine white powder of −325 mesh from Sigma-Aldrich as MgO and a fine yellow powder of ammonium phosphomolybdate hydrate produced by Kanto as the POM to incorporate as adsorbents into nanofibrous protective materials against CWAs.

Nanofibrous outer layer for repellent protection against CWA simulants

We introduced the selected absorbents (MgO and POM) onto the surface of mANF using the SEE process, which effectively deposited the absorbents on the surface of the nanofibres. The as-prepared MgO/mANF and POM/mANF composite nanofibre mats were washed to remove the LiCl salt, which prevented crystallization of Nomex. The composite nanofibres were then heat-treated to induce crystallization, which enhanced their chemical stability and mechanical properties. An amphiphobic outer layer was produced by post-treatment with a fluorinated water and oil repellent to give [O]MgO/mANF and [O]POM/mANF.

The pristine Nomex nanofibres produced by electrospinning had a uniform diameter of 207 ± 54 nm and form uniaxially aligned arrays (Fig. S6). In the case of the nanofibre composites containing the adsorbents, MgO and POM were dispersed on and between the nanofibres, as illustrated in Fig. 1 and S7. The alignment of the nanofibres was preserved despite the presence of the adsorbents. In addition, it is possible to change the content of the adsorbents in the composite nanofibres by regulating SEE conditions such as concentration and flow rate. To determine the thermal properties of the composite nanofibres and their adsorbent content, DTA/TGA was conducted in N2 at a heating rate of 10 °C min−1. As shown in Fig. 2, the neat Nomex nanofibres showed a dramatic weight loss around 465 °C (see the inset), and the as-prepared composite nanofibres showed similar thermal degradation behavior. The thermal behavior of the MgO- and POM-incorporated composite nanofibres was similar. The adsorbent content of the composite nanofibres was 14.1 ± 0.5%, which was calculated from the ratio of the nanofibres to adsorbent. The temperatures at 10% weight loss (Td10) and dramatic weight loss reveal that the surface-incorporated adsorbents did not directly affect to the thermal properties of the composite nanofibres. In contrast, the composite nanofibres treated with the fluorinated water and oil repellent ([O]MgO/mANF) displayed different thermal degradation behavior. [O]MgO/mANF showed progressive weight loss in the temperature range of 250–400 °C. This weight loss originated from the thermal degradation of the fluorinated water and oil repellent. Comparison of the three components at 700 °C allowed us to determine that the content of repellent in [O]MgO/mANF was 15.1 ± 0.3%.


image file: c6ra23826b-f1.tif
Fig. 1 Morphology of (a and b) MgO/mNAF and (c and d) POM/mANF nanofibre composites used as outer layers of nanofibrous protective materials.

image file: c6ra23826b-f2.tif
Fig. 2 Differential thermal analysis (inset) and thermal gravimetric analysis of neat mANF, as-prepared MgO/mANF, and [O]MgO/mANF.

To estimate the protective performance of composite nanofibres against liquid CWAs, the surface wettability or non-wettability of the composite nanofibres was evaluated using WCA and OCA measurements with water and CWA simulants (2-CEES and DMMP), respectively. The contact angle is the angle formed between the tangent plane to the surface of the nanofibres and the tangent plane to the surface of the liquid droplet at the point of intersection,33 and reflects the wettability of the nanofibres. As depicted in Fig. 3, the as-prepared MgO/mANF quickly absorbed both water and simulants (data not shown for mANF). This indicates that the nanofibres originally have high affinity for both water and oil. In contrast, the nanofibre mats treated with fluorinated water and oil repellent exhibited an amphiphobic nature. The mANF treated with the repellent showed high hydrophobicity (WCA > 120°) and oleophobicity (OCA > 90°), but these properties were not strong enough to repel the CWAs effectively from the outside. The composite nanofibre mat with the adsorbents exhibited both superhydrophobicity (WCA greater than 150°) and high oleophobicity (OCA higher than 120°). We believe that the modified surface roughness of the nanofibre mats with and without adsorbents induced the difference between their non-wettable surfaces. The geometric structure of a surface has been identified as one of the most important factors that affects surface wettability,34 and high surface roughness is essential to develop non-wettable surfaces. In the case of the composite nanofibre mats, the adsorbents were incorporated on the surface of the nanofibres and nanofibre mats, so the composite nanofibre mats had rougher surfaces than the pristine Nomex nanofibre mat. This increase of surface roughness enhanced the amphiphobicity of the composite nanofibre mats compared with that of the mANF.


image file: c6ra23826b-f3.tif
Fig. 3 Amphiphobic surface behavior of [O]MgO/mANF and [O]POM/mANF.

Nanofibrous inner layer for adsorptive protection against CWA simulants

[I]MgO/PANF and [I]POM/PANF nanofibre composites were prepared as the inner layer of protective clothing using the SEE process, which effectively deposited the adsorbents MgO and POM onto the surface of PANF. The morphology of the nanofibres was observed by FE-SEM. The pristine PANF were disordered, and formed a continuous shape without defects that had a smooth surface with a uniform diameter of 163 ± 21 nm (Fig. S8). In contrast, [I]MgO/PANF and [I]POM/PANF contained electrosprayed MgO and POM, respectively, on and between the nanofibres without the formation of large aggregates, as illustrated in Fig. 4. The uniform morphology and disordered array of nanofibres was preserved despite the presence of adsorbents. The adsorbent content could be changed by controlling SEE conditions like concentration and flow rate. TGA was conducted to determine the thermal properties and absorbent contents of the composite nanofibres, as shown in Fig. 5.
image file: c6ra23826b-f4.tif
Fig. 4 Morphology of (a and b) [I]MgO/PANF and (c and d) [I]POM/PANF nanofibre composites used as inner layers of nanofibrous protective materials.

image file: c6ra23826b-f5.tif
Fig. 5 Thermal degradation behavior of neat polyamide 66 nanofibres (PANF), [I]MgO/PANF and [I]POM/PANF nanofibre composites.

Neat PANF showed a Td10 of around 370 °C and dramatic weight loss around 400 °C. [I]MgO/PANF and [I]POM/PANF, which had absorbent contents of 18.1 and 16.4 wt%, respectively, showed similar thermal degradation behavior to that of PANF. This indicates that the adsorbents located on the surface of the nanofibres had little effect on their thermal behavior.

Tensile tests were conducted to determine the mechanical properties of the PANF composites. As shown in Table S1, the surface-incorporated adsorbents had little effect on the mechanical properties, such as the Young's modulus, tensile stress and tensile strain, of the nanofibres. The adsorbents located on the surface of the nanofibres did not improve their mechanical properties, unlike ordinary composites that contain fillers inside the nanofibres.35,36 However, the adsorbents on the nanofibre surface did affect the flow pore diameter and pore size distribution of the nanofibre mats. The pore characteristics of PANF and [I]MgO/PANF were observed by capillary flow porometry (liquid extrusion flow porometry) as shown in Fig. S9. During capillary flow porometry measurements, the pores of the nanofibre mats were spontaneously filled with a wetting liquid and then the liquid was extruded from the pores by a non-reacting gas, such as N2.

The differential pressure is related to pore diameter according to D = 4γ[thin space (1/6-em)]cos[thin space (1/6-em)]θ/p, where D is flow pore diameter, γ is the surface tension of the wetting liquid, θ is the contact angle of the wetting liquid and p is differential pressure.37–39 The pores of the nanofibre mat were filled with a wetting liquid, and the liquid was removed by pressurized N2 gas allowed to flow through the empty pores. The adsorbents on the nanofibre surface decreased the mean flow pore diameter of [I]MgO/PANF (0.139 μm) compared with that of PANF (0.150 μm). The pore volume was also decreased by the presence of adsorbent. The smaller flow pore diameter caused the air permeability to decrease, as summarized in Table 2. In the case of WVTR, the composite nanofibre mats [I]MgO/PANF and [I]POM/PANF showed similar water vapor permeability compared with that of neat PANF. These results indicate that the decrease of flow pore diameter influences the air permeability more than the water vapor permeability of the composite nanofibre mats. These results indicate that the nanofibre composites should be able to improve the problem of moisture retention affecting the protective clothing currently used by the Korean Army.

Table 2 Air permeability and water vapor transmittance rate of inner layers
Material PANF [I]MgO/PANF [I]POM/PANF
a ASTM D737, test pressure 125 Pa, test area 38 cm2.b ASTM E96, 40% RH, 40 ± 1 °C.
Air permeabilitya (cfm) 0.358 ± 0.008 0.306 ± 0.004 0.261 ± 0.020
Water vapor transmission rateb (g per m2 per day) 4863 ± 101 4575 ± 35 4722 ± 52


To investigate the resistance of the composite nanofibre mats to permeation by gas CWAs, permeation tests were conducted using the simulants 2-CEES and DMMP. Table 3 shows the relative amounts of the simulants that penetrated through PANF, [I]MgO/PANF and [I]POM/PANF. The composite nanofibre mats showed slightly better performance than PANF, but were not sufficiently effective to protect users from the CWAs. A single sheet of the composite nanofibre mat (91 μm thick) was ineffective to adsorb the passing simulant gas. On closer scrutiny, in the direct contact-type experiments (see Fig. S3), the simulant gas passed directly through the nanofibre mat, so the captured amount of simulant was larger than that in the dynamic diffusion-type experiments regardless of the small amount of simulant gas that passed through the mat (1000 cm3 vs. 2000 cm3). In addition, 2-CEES penetrated into the nanofibre mats more than DMMP. This is attributed to the higher volatility of 2-CEES than DMMP. Because a single layer of the composite nanofibre mats would not effectively protect a user from CWAs, we decided to use several sheets of the composite nanofibre mats as the inner layer of materials to achieve acceptable protection against CWAs.

Table 3 Permeation test of the simulant of chemical warfare agents through the inner layer
CWA simulant Blank PANF [I]MgO/PANF [I]POM/PANF
Direct contact
2-CEES (μg m−3) 40.14, 100% 25.88, 64.5% 12.97, 32.3% 10.65, 26.5%
DMMP (μg m−3) 62.76, 100% 17.96, 28.6% 5.76, 9.2% 4.99, 7.8%
[thin space (1/6-em)]
Dynamic diffusion
2-CEES (μg m−3) 30.96, 100% 6.56, 21.2% 2.56, 8.3% 2.02, 6.5%
DMMP (μg m−3) 37.76, 100% 6.68, 17.7% 4.80, 12.7% 2.64, 7.0%


Assembly of outer and inner layers to form nanofibrous protective materials against CWA simulants

The numbers of outer and inner layers were coordinated to compare the protection ability of the assemblies against CWAs according to thickness. Also, to compare the effectiveness of the adsorbents (MgO and POM), outer and inner layers containing the same adsorbent were paired. In particular, it was desired that the outer layer based on mANF should contain at least two layers because mANF aligned in the same direction. The mANF mats showed excellent mechanical properties along the alignment direction, but not along the transverse direction. Controlling the layer stacking allowed the overall performance of the assemblies to be regulated. The repellent nature of the outer layers prevents invasion of the assemblies by the liquid CWA. Meanwhile, the adsorbents in the inner layers are expected to restrain penetration of gas CWAs.

Physical properties, such as thickness, weight per area, cool/warm feeling and air/moisture permeability, of each assembly were compared with those of the permeable protective clothing of the Korean Army that is currently being used as chemical protective gear as a reference. The physical properties of each assembly strongly depended on the number of stacked layers, which allowed the desired properties of the assemblies to be improved by layer stacking. As listed in Table 4, the thickness and weight per area of the assemblies increased with layer number. In the case of the assembly composed of two outer layers and six inner layers, the thickness and weight of the assembly were similar to those of the reference material. Therefore, to lighten the weight of the assemblies compared with that of currently used permeable protective clothing, the number of layers in the assemblies was limited to a maximum of eight.

Table 4 Weight, thickness and maximum heat transfer rate (qmax) of assemblies
  Nanofibrous outer/inner layers with MgO or POM Outer/inner layers of permeable protective clothing used by the Korean Army
Number of sheets Thickness (μm) Weight per area (g m−2) Maximum heat transfer rate, qmax (W cm−2) Thickness (μm) Weight per area (g m−2) Maximum heat transfer rate, qmax (W cm−2)
Outer layer (O) 1 75 33 0.126 0.380 260 0.161
2 137 65 0.123
Inner layer (I) 1 91 62 0.145 1300 360 0.092
2 166 125 0.143
Assembly (O + I) 2 O + 2 I 415 285 0.124 1700 620 0.087
2 O + 4 I 542 423 0.121
2 O + 6 I 681 581 0.116
2 O + 8 I 817 653 0.110


The cool/warm feeling of a material can be evaluated by qmax. Cool/warm feeling represents the transfer of heat from a body to a sample of lower temperature. The magnitude of heat transferred after 0.2 s from the moment the sample contacts with the heated body was converted to qmax, which may increase or decrease depending on the sample. If qmax increases, it indicates that the material feels cold and vice versa. Table 4 lists qmax of the assemblies with various thicknesses. There was little difference between qmax of assemblies containing MgO and POM with the same thickness. The cool feeling of the assemblies decreased as their thickness increased with raising layer number. However, the nanofibrous materials gave a cooler feeling than reference material O-KA according to comparison of qmax of O-KA (0.154 W cm−2) with those of single sheets of outer/inner layer and the assembly with two outer and two inner layers, which was even thicker than O-KA. This indicates that heat transfers rapidly from the nanofibres to a solid. The assembly composed of two outer and six inner layers showed a cooler feeling compared with that of currently used permeable protective clothing. The inner layer of the reference clothing (I-KA) had a great effect on cool/warm feeling than the outer layer because I-KA was formed of a thick polyurethane foam (1.3 mm), which contained a considerable amount of air. These results show that the assemblies made of the composite nanofibre mats should feel cooler to wear than the currently used protective clothing.

To estimate the gas transfer through the protective clothing materials, the air and water vapor permeability of assemblies with different compositions and thicknesses were compared with those of currently used permeable protective clothing (Table 5). The reference protective clothing showed the higher air permeability than the assemblies, because the outer layer was made of a woven fabric with warp and weft threads, and the inner layer was made of porous polyurethane foam. In contrast, the assemblies consisted of nonwoven nanofibre mats, so they exhibited extremely low air permeability of less than 0.5 cfm. The nanofibre mats in the assemblies have a small fibre diameter of less than 300 nm and pores with a mean flow pore size of 140 nm. An interesting complicating factor in the analysis of air permeability through the assemblies occurs when the mean free path of air becomes comparable to the fibre size.40 Because of air spin at the nanofibre surface, the normal linear dependence of air permeability with pressure drop is less applicable to the air flow field in pores. The pressure drop predicted by assuming continuous flow through beds of fibres is lowered by a one third for a fibre with a diameter of 100 nm.41 However, regarding water vapor transport, although the assemblies showed low air permeability, they exhibited excellent water vapor transport. In particular, the assemblies composed of two outer and six inner layers had similar water vapor permeability to the reference protective clothing. The water vapor permeability of the assemblies consisting of two outer and eight inner layers or more was much lower than that of the reference clothing. Based on the results of the air and water vapor permeability measurements, the assemblies should provide good resistance to the penetration of CWAs in gas form while still allowing water vapor transmission to promote evaporative cooling of the body. The composite nanofibre mats have a porous structure with a mean flow pore diameter of about 140 nm. Their resistance to air flow is quite large because of the small diameter of the flow pores in the assemblies. However, the high resistance to air flow does not impede the diffusion of moisture through the pore structure of the nanofibre mat. These results suggest that the assemblies are promising candidates for protective clothing materials because of their high rates of water vapor transmission and low air flow.

Table 5 Air permeability and water vapor transmission of assemblies
  Number of sheets MgO-containing outer or inner layers POM-containing outer or inner layers Permeable protective clothing used by the Korean Army
Air permeability (cfm) Water vapor transmission (g per m2 per 24 h) Air permeability (cfm) Water vapor transmission (g per m2 per 24 h) Air permeability (cfm) Water vapor transmission (g per m2 per 24 h)
Outer layer (O) 1 0.534 4809 0.503 4675 5.41 4342
2 0.272 4748 0.267 4480
Inner layer (I) 1 0.261 4575 0.306 4722 60.7 3623
2 0.126 4282 0.152 4331
Assembly (O + I) 2 O + 2 I 0.062 4062 0.068 4229 4.27 3292
2 O + 4 I 0.057 3662 0.064 3809
2 O + 6 I 0.032 3229 0.036 3494
2 O + 8 I 0.026 2188 0.030 2276


Based on the results of the air and water vapor permeability measurements, the assemblies should provide good resistance to the penetration of CWAs in gas form while still allowing water vapor transmission to promote evaporative cooling of the body. The composite nanofibre mats have a porous structure with a mean flow pore diameter of about 140 nm. Their resistance to air flow is quite large because of the small diameter of the flow pores in the assemblies. However, the high resistance to air flow does not impede the diffusion of moisture through the pore structure of the nanofibre mat. These results suggest that the assemblies are promising candidates for protective clothing materials because of their high rates of water vapor transmission and low air flow.

To estimate the protective performance of the assemblies against liquid CWAs, their surface wettability was evaluated using WCA and OCA measurements with water, 2-CEES and DMMP. The surface wettability of the outer layer of the reference protective clothing O-KA was measured in the same way for comparison with that of the assemblies. The samples possessed an amphiphobic nature, as shown in Fig. 6. O-KA displayed both hydrophobicity with a WCA higher than 120° and oleophobicity. The assemblies simultaneously exhibited superhydrophobicity (WCA greater than 150°) and high oleophobicity (OCA higher than 120°). We believe that the difference of wettability between the assemblies and O-KA can be attributed to the surface roughness of the samples.34 The outer layer of each assembly contained the adsorbents MgO and POM on the surface of nanofibres and nanofibre mats, so it had a rougher surface than that of O-KA. The increase of surface roughness was essential to develop non-wettable surfaces. The increase of roughness induced by the adsorbents improved the ability of the assembly to protect against CWA simulants.


image file: c6ra23826b-f6.tif
Fig. 6 Amphiphobic surface behavior of the outer layer of permeable protective clothing used by the Korean Army (O-KA), and assemblies containing MgO and POM as nanofibrous protective materials against CWA simulants 2-CEES and DMMP.

To investigate the resistance of the assemblies to permeation by gas CWAs, permeation tests were conducted according to the TOP 08-2-501 standard using the simulants 2-CEES and DMMP. The penetration behavior of the simulants through each assembly was profiled by measuring the amount of simulant that passed through the assembly at regular intervals, as shown in Fig. S10. Evaporated 2-CEES gas rapidly passed through the assembly and all of the gas had penetrated though the assembly after 6 h room temperature. In the case of DMMP, the gas passed slowly and continuously through the sample for 12 h. These results were attributed to the difference in volatility between 2-CEES and DMMP; 2-CEES shows much higher relative volatility (<3.4 mmHg vapor pressure at 25 °C, 16[thin space (1/6-em)]570 mg m−3 volatility at 20 °C) than DMMP (∼1 mmHg vapor pressure at 25 °C, 347 mg m−3 volatility at 20 °C). The penetration behavior of simulants was similar for the assemblies with POM and the reference protective clothing (data not shown). Table 6 lists the relative amounts of the simulants that penetrated through the reference protective clothing and assemblies with MgO and POM. The assembly with two outer and eight inner sheets was excluded from the evaluation because it showed poorer performance in terms of weight density and moisture permeability than the reference material. The reference protective clothing currently used by the Korean Army exhibited permeabilities of 383 μg cm−2 for 2-CEES and 186 μg cm−2 for DMMP after 12 h. These results are similar to those obtained for the assembly containing MgO with two outer and four inner sheets, indicating that the assembly had a comparable level of protection ability to the protective clothing despite its thinner thickness and lighter weight. In addition, the assembly exhibited better moisture permeability and cool/warm feeling than the reference protective clothing. The assembly containing POM with two outer and four inner sheets showed higher protection ability than the reference protective clothing. These results indicate that the assemblies based on nanofibrous composites can be used to make lighter protective clothing materials than those currently available. Furthermore, the assembly with two outer and six inner sheets, which had comparable weight density to that of the reference protective clothing, exhibited improved protection ability against the simulants. This means that although only one layer of nanofibrous material does not achieve protection ability, assemblies of laminated nanofibre layers can attain more effective protection against CWAs than the currently used permeable protective clothing.

Table 6 Permeability of CWA simulants through assemblies
    Assembly with outer and inner layers containing MgO Assemblies with outer and inner layers containing POM Permeable protective clothing used by the Korean Army
2-CEES penetration (μg cm−2) DMMP penetration (μg cm−2) 2-CEES penetration (μg cm−2) DMMP penetration (μg cm−2) 2-CEES penetration (μg cm−2) DMMP penetration (μg cm−2)
Assembly with outer layers (O) and inner layers (I) 2 O + 2 I 772.25 323.67 744.82 311.12 382.99 185.52
2 O + 4 I 362.53 126.30 178.21 60.38
2 O + 6 I 251.71 108.72 161.53 52.65


Conclusions

The objective of this study was to develop permeable nanofibrous materials for used as protective clothing against CWAs. To prevent the invasion of liquid CWAs, amphiphobic nanofibre composites were applied as outer layers. The outer layers were not wetted by water, 2-CEES and DMMP. Inner layers, designed to adsorb gaseous CWAs, showed better adsorption of CWA simulants than that of a neat PANF, but the use of a single layer was inadequate to protect from CWAs. Therefore, assemblies, composed of several sheets of outer and inner layers, were fabricated by a spray- and heat-bonding process in order to improve the protection ability of the inner layers against CWAs. The properties of the assemblies, such as thickness, weight density, air/moisture permeability, cool/warm feeling and protection ability, can be controlled by the number of stacked sheets. As a result, the assemblies can provide good protection against CWAs, while still allowing considerable water vapor transmission to promote evaporative cooling of the body. These assemblies can be used as a protective material against various contaminants such as organic pollutants and harmful particulates, as well as against CWAs. Our results will enable the design and production of permeable protective clothing with superior performance to that currently available.

Acknowledgements

This research was supported by the Defense Acquisition Program Administration (DAPA) and by the Agency for Defense Development (ADD).

Notes and references

  1. NATO Handbook on the Medical Aspects of NBC Defensive Operations, Department of the Army, Washington, DC, 1996 Search PubMed.
  2. L. Szinicz, Toxicology, 2005, 214, 167 CrossRef CAS PubMed.
  3. E. F. G. Dickson, J. Toxicol. Environ. Health, Part A, 2008, 71, 1382 CrossRef PubMed.
  4. P. Gao, W. P. King and R. J. Shaffer, J. Occup. Environ. Hyg., 2007, 4, 562 CrossRef CAS PubMed.
  5. T. Pal, G. D. Griffin, G. H. Miller, A. P. Watson, M. L. Daugherty and T. Vodinh, J. Hazard. Mater., 1993, 33, 123 CrossRef CAS.
  6. D. K. Liu, R. W. Wannemacher, T. H. Snider and T. L. Hayes, J. Appl. Toxicol., 1999, 17, S41 Search PubMed.
  7. E. Wilusz, Military Textiles, Woodhead Publishing Limited, England, 2008 Search PubMed.
  8. S. Sundarrajan and S. Ramakrishna, J. Mater. Sci., 2007, 42, 8400 CrossRef CAS.
  9. G. W. Wagner, P. W. Bartram, O. Koper and K. J. Klabunde, J. Phys. Chem. B, 1999, 103, 3225 CrossRef CAS.
  10. T. H. Mahato, G. K. Prasad, B. Singh, K. Batra and K. Ganesan, Microporous Mesoporous Mater., 2010, 132, 15 CrossRef CAS.
  11. T. H. Mahato, G. K. Prasad, B. Singh, J. Acharya, A. R. Srivastava and R. Vijayaraghavan, J. Hazard. Mater., 2009, 165, 928 CrossRef CAS PubMed.
  12. G. K. Prasad, T. H. Mahato, B. Singh, K. Ganesan, P. Pandey and K. Sekhar, J. Hazard. Mater., 2007, 149, 460 CrossRef CAS PubMed.
  13. D. A. Panayotov and J. R. Morris, J. Phys. Chem. C, 2009, 113, 15684 CAS.
  14. R. Ramaseshan and S. Ramakrishna, J. Am. Ceram. Soc., 2007, 90, 1836 CrossRef CAS.
  15. Ş. Neaţu, V. I. Pârvulescu, G. Epure, N. Petrea, V. Şomoghi, G. Ricchiardi, S. Bordiga and A. Zecchina, Appl. Catal., B, 2009, 91, 546 CrossRef.
  16. M. Grandcolas, L. Sinault, F. Mosset, A. Louvet, N. Keller and V. Kellera, Appl. Catal., A, 2011, 391, 455 CrossRef CAS.
  17. B. Cojocaru, Ş. Neaţu, V. I. Pârvulescu, V. Şomoghi, N. Petrea, G. Epure, M. Alvaro and H. Garcia, ChemSusChem, 2009, 2, 427 CrossRef CAS PubMed.
  18. Ş. Neaţu, B. Cojocaru, V. I. Pârvulescu, V. Şomoghi, M. Alvaro and H. Garcia, J. Mater. Chem., 2010, 20, 4050 RSC.
  19. B. M. Smith, Chem. Soc. Rev., 2008, 37, 470 RSC.
  20. O. Koper, E. Lucas and K. J. Klabunde, J. Appl. Toxicol., 1999, 19, S59 CAS.
  21. M. K. Ferguson-McPherson, E. R. Low, A. R. Esker and J. R. Morris, Langmuir, 2005, 21, 11226 CrossRef CAS PubMed.
  22. N. M. Okun, J. C. Tarr, D. A. Hilleshiem, L. Zhang, K. I. Hardcastle and C. L. Hill, J. Mol. Catal. A: Chem., 2006, 246, 11 CrossRef CAS.
  23. R. D. Gall, C. L. Hill and J. E. Walker, J. Catal., 1996, 159, 473 CrossRef CAS.
  24. S. Agarwal, A. Greiner and J. H. Wendorff, Prog. Polym. Sci., 2013, 38, 963 CrossRef CAS.
  25. J.-M. Li, D.-P. Wei, Y.-B. Hu, F. Jie and Z.-A. Xu, CrystEngComm, 2014, 16, 964 RSC.
  26. J.-M. Li, X.-L. Zeng, D.-P. Wei, Y.-B. Hu and Z.-A. Xu, ACS Appl. Mater. Interfaces, 2014, 6, 4490 CAS.
  27. R. Ramaseshan, S. Sundarrajan, Y. Liu, R. S. Barhate, N. L. Lala and S. Ramakrishna, Nanotechnology, 2006, 17, 2947 CrossRef CAS.
  28. H. L. Schreuder, P. Gibson, K. Senecal, M. Sennett, J. Walker, W. Yeomans, D. Ziegler and P. T. Tsai, J. Adv. Mater., 2002, 34, 44 Search PubMed.
  29. ASTM D5160-95, Standard Guide for Gas-Phase Adsorption Testing of Activated Carbon, American Society for Testing and Materials (ASTM) International, West Conshohocken, 2008 Search PubMed.
  30. S.-Y. Ryu, J. W. Chung and S.-Y. Kwak, Compos. Sci. Technol., 2015, 117, 9 CrossRef CAS.
  31. M. Yoneda and S. Kawabata, J. Text. Mach. Soc. Jpn., 1985, 31, 79 Search PubMed.
  32. Test Operations Procedure 8-2-501, Permeation and Penetration of Air-permeable, Semipermeable and Impermeable Materials with Chemical Agents or Simulants (Specimen Testing), U.S. Army Dugway Proving Ground, UT, March 1997, unclassified report AD A322329 Search PubMed.
  33. H. Y. Erbil, Surface Chemistry of Solid and Liquid Interfaces, Wiley-Blackwell, Oxford, 2006 Search PubMed.
  34. J. Zhao, C. Dai, J. Fang, X. Feng, L. Yan and M. Zhao, Colloids Surf., A, 2014, 448, 93 CrossRef.
  35. S. Sundarrajan and S. Ramakrishna, J. Mater. Sci., 2007, 42, 8400 CrossRef CAS.
  36. Y. Ding, P. Zhang, Y. Jiang, F. Xu, J. Yin and Y. Zuo, Mater. Lett., 2009, 63, 34 CrossRef CAS.
  37. A. Jena and K. Gupta, A Novel Technique for Pore Structure Characterization Without the Use of Any Toxic Material, Nondestructive Characterization of Materials XI, Springer, New York, 2002 Search PubMed.
  38. A. Jena and K. Gupta, Fluid/Part. Sep. J., 2002, 14, 227 Search PubMed.
  39. A. Jena and K. Gupta, J. Power Sources, 1999, 80, 46 CrossRef CAS.
  40. A. A. Kirsch, I. B. Stechkina and N. A. Fuchs, Aerosol Sci., 1974, 5, 39 CrossRef.
  41. W. Hinds, Aerosol Technology, Wiley, New York, 1982 Search PubMed.

Footnote

Electronic supplementary information (ESI) available: Mechanical properties of pristine polyamide 66 nanofibre and composite nanofibre mats for inner layer; schematic representation of the simultaneous electrospinning and electrospraying process; DSC curves of meta-aramid nanofibre; schematic representations of the permeation experimental systems used to investigate the resistance of the nanofibre composites against gas CWA simulants and fabrication of assemblies of composite nanofibre mats; flow pore characteristics of the nanofibre mats; morphology of pristine meta-aramid and polyamide 66 nanofibres; EDS mapping image of nanofibre composites for outer layer; penetration behavior of CWA simulants through assemblies. See DOI: 10.1039/c6ra23826b

This journal is © The Royal Society of Chemistry 2017