Mohamed Gamal
Mohamed
,
Kuo-Chih
Hsu
,
Jin-Long
Hong
and
Shiao-Wei
Kuo
*
Department of Materials and Optoelectronic Science, Center for Nanoscience and Nanotechnology, National Sun Yat-Sen University, Kaohsiung, 804, Taiwan. E-mail: kuosw@faculty.nsysu.edu.tw
First published on 20th October 2015
In this study, we synthesized unusual fluorescent polyhedral oligomeric silsesquioxane (POSS)-containing polymers lacking any common fluorescent units (e.g., phenyl or heterocyclic rings): a poly(maleimide isobutyl POSS) [poly(MIPOSS)] homopolymer and poly(styrene-alt-maleimide isobutyl POSS) [poly(S-alt-MIPOSS] and poly(4-acetoxystyrene-alt-maleimide isobutyl POSS) [poly(AS-alt-MIPOSS)] alternating copolymers, through free radical polymerization, and a poly(4-hydroxystyrene-alt-maleimide isobutyl POSS) [poly(HS-alt-MIPOSS)] alternating copolymer, through acetoxy hydrazinolysis of poly(AS-alt-MIPOSS). We used 1H, 13C, and 29Si nuclear magnetic resonance spectroscopy, Fourier transform infrared (FTIR) spectroscopy, and MALDI-TOF mass spectrometry to examine the chemical structures and sequence distributions of these POSS-containing polymers. The FTIR spectra revealed the existence of specific intermolecular interactions, namely dipole–dipole interactions between the CO groups in poly(MIPOSS) and poly(AS-alt-MIPOSS) and intermolecular hydrogen bonding between the C
O groups of the MIPOSS units and the OH groups of the HS units in poly(HS-alt-MIPOSS). Differential scanning calorimetry and thermogravimetric analyses revealed that the incorporation of MIPOSS units could enhance the thermal stability, but decrease the glass transition temperatures, of these alternating copolymers. The photoluminescence emission of poly(MIPOSS) was greater than those of the POSS-containing alternating copolymers, presumably because of the former's crystallinity and clustering of locked C
O groups of POSS units.
Most fluorescent polymeric materials feature π-aromatic units (benzene or heterocyclic rings) as emissive units.15,16 Recently, fluorescent polymers lacking such conventional fluorescent units have attracted much attention for their excellent biocompatibility and biodegradability. For example, Tang et al. also found that polymerization of nonluminescent monomers – through free radical polymerization, reversible addition/fragmentation chain transfer (RAFT), or atom transfer radical polymerization – lacking luminescent groups can also give highly emissive polymeric materials.15,16 In addition, Tang and coworkers observed that alternating poly(vinyl acetate-alt-maleic anhydride) nanoparticles exhibited strong light emission and AIE effects because of intermolecular interactions between their five membered dihydrofuran-2,5-dione groups or clustering of their locked CO groups.16 In addition, hyperbranched polymers featuring tertiary amino units, including polyureas,17 poly(ether amide)s,18 poly(amido amine)s,19 and poly(amino ester)s,20 can act as luminescent polymers. The emission mechanism of these materials originates from the presence of the tertiary amino moieties.21,22 Succinimide derivatives are known fluorescence quenchers of proteins, and maleic anhydride-containing polymers can display fluorescence.23 Polyisobutene succinic anhydrides and their imides have displayed unexpected emissions that have been attributed to the AIE effects of their C
O groups.24
Polyhedral oligomeric silsesquioxane (POSS) and its derivatives comprise an intriguing class of compounds that can be considered as nanostructured inorganic composites or organic/inorganic hybrid materials.25–30 POSS derivatives have been studied in academic and industrial fields because of their interesting interfacial interactions; they have well-defined cubic three-dimensional cage-like structures with a chemical formula (RSiO1.5)8, where the R unit is an organic group that can impart solubility and compatibility within a polymer matrix – indeed, the introduction of POSS moieties into polymer matrices can result in novel polymers displaying interesting mechanical properties, high thermal stabilities, and low flammability.31–35 Hayakawa and Gopalan successfully synthesized the polystyrene-b-PMAPOSS (poly(methacrylate POSS) diblock copolymers with well-defined molecular distributions and high degrees of polymerization; these polymers exhibited microphase-separated structures.36–38 Monticelli et al. grafted a titanium-containing POSS (M-POSS) to the maleic anhydride groups of a poly(styrene-alt-maleic anhydride) copolymer; the resulting nanofiber/M-POSS system displayed good photocatalytic activity for the degradation of sulforhodamine B, an organic dye.39 Recently, Zhang et al. synthesized the alternating copolymer poly(styrene-alt-maleimide isobutyl POSS) [poly(S-alt-MIPOSS)] through RAFT polymerization, finding that incorporation of the MIPOSS moieties greatly enhanced the thermal properties of the copolymers.40 Zhang et al. also demonstrated that poly[MIPOSS-alt-vinylbenzyl poly(ethylene glycol)] [poly(MIPOSS-alt-VBPEG)] could self-assemble in aqueous solution to form spherical structures.41
In this study, we synthesized a poly(MIPOSS) homopolymer and POSS-containing poly(S-alt-MIPOSS) and poly(AS-alt-MIPOSS) alternating copolymers through facile and ordinary free radical polymerizations in the presence of AIBN as the initiator in THF solution. We then prepared a poly(HS-alt-MIPOSS) alternating copolymer through acetoxy hydrazinolysis of poly(AS-alt-MIPOSS) using hydrazine monohydrate in 1,4-dioxane (Scheme 1). 1H, 13C, and 29Si NMR spectroscopy, MALDI TOF mass spectrometry, and Fourier transform infrared (FTIR) spectroscopy confirmed their chemical structures. Furthermore, we employed differential scanning calorimetry (DSC) and thermogravimetric analysis (TGA) to determine the thermal degradation temperatures, char yields, and glass transition temperatures of the POSS-containing homopolymer and the alternating copolymers. FTIR spectra revealed the existence of specific intermolecular interaction, including dipole–dipole and hydrogen bonding interactions, in these POSS-containing polymers. We used wide-angle X-ray diffraction (WAXD) to examine the crystallinity of these POSS-containing polymers, and photoluminescence (PL) spectroscopy to study the optical properties of our POSS-containing alternating copolymers in solution and in the bulk state. To the best of our knowledge, we are the first to report the unusual fluorescent polyhedral oligomeric silsesquioxane (POSS)-containing polymers (poly(maleimide isobutyl POSS) lacking any common fluorescent unit by a simple free radical polymerization and study their emission behavior in the solid and solution states. In addition, we expect that these fluorescent alternating polymeric materials containing POSS nanoparticles can result in dramatic improvements in the physical properties such as a reduction in flammability and oxidation resistance.
![]() | ||
Scheme 1 Chemical structures and peak assignments for NMR spectra of poly(S-alt-MIPOSS), poly(AS-alt-MIPOSS) and poly(HS-alt-MIPOSS) copolymers. |
Sample |
M
n![]() |
PDIa |
M
n![]() |
PDIb |
T
g![]() |
λ
ab![]() |
Quantum yielde (%) |
---|---|---|---|---|---|---|---|
a Measured by MALDI-TOF MS analysis. b Measured by GPC. c Measured by DSC. d Determined by UV-vis absorption measurement. e Determined by using an integrated sphere by Ocean Optics. | |||||||
MIPOSS | 2544.1 | 1.08 | 2110 | 1.33 | — | 237.3/280.0 | 72.5 |
S-alt-MIPOSS | 3887.9 | 1.12 | 14![]() |
1.98 | 103 | 236.0/259.3 | 55.5 |
AS-alt-MIPOSS | 2915.4 | 1.16 | 6570 | 1.64 | 75 | 235.7/262.5 | 46.8 |
HS-alt-MIPOSS | 3155.9 | 1.16 | 5370 | 1.88 | 96 | 236.1/278.7 | 7.0 |
![]() | ||
Fig. 1 1H NMR spectra of (a) poly(MIPOSS), (b) poly(S-alt-MIPOSS), (c) poly(AS-alt-MIPOSS), and (d) poly(HS-alt-MIPOSS) in CDCl3. |
Fig. 2 displays the 13C NMR spectra of these four polymeric compounds. The 13C NMR spectrum of poly(MIPOSS) in CDCl3 at room temperature [Fig. 2(a)] features signals at 177.96, 41.28, and 9.45 ppm, representing the resonances of the carbon nuclei of the CO groups, the SiCH2CH2CH2N methylene unit, and the SiCH2CH(CH3)2 methine unit, respectively. The spectrum of poly(S-alt-MIPOSS) [Fig. 2(b)] features an additional signal centered at 129.15 ppm, representing the carbon nuclei of the aromatic units. The signals of poly(AS-alt-MIPOSS) [Fig. 2(c)] appear at 179.07, 170.05, 151.23–123.01, and 21.40 ppm, corresponding to the imide C
O, acetyl C
O, aromatic, and OCOCH3 methyl groups, respectively. In Fig. 2(d), the absence of the signal (170.05 ppm) of the C
O group of the acetate units and the shifts of the signals of the carbon nuclei of the aromatic rings, to 156.09 (PhOH, peak o) and 116.66 (peak n) ppm, confirmed the synthesis of poly(HS-alt-MIPOSS). Scheme 1 summarizes the other peak assignments. We could also use 13C NMR spectroscopy to investigate the alternating copolymers of the maleimide isobutyl POSS and styrene derivatives; the signals of the quaternary carbon nuclei in the aromatic styrene units appear at 151.23–123.01 ppm, indicating that the sequence structures of the copolymers were non-alternating, semi-alternating, and alternating.40,43,44Fig. 3 presents the 29Si NMR spectra of poly(MIPOSS), poly(S-alt-MIPOSS), poly(AS-alt-MIPOSS), and poly(HS-alt-MIPOSS) in CDCl3. Two peaks appear, centered at −54.02 (peak a) and −54.44 ppm (peak b), corresponding to their OSiCH2CH2CH2N and OSiCH2CH(CH3)2 units, respectively. These 29Si NMR spectra suggest that no cage cleavage occurred during the free radical polymerization, with the POSS cores remaining intact. Taken together, the NMR spectra are consistent with the chemical structures of the homopolymer and alternating copolymers.
![]() | ||
Fig. 2 13C NMR spectra of (a) poly(MIPOSS), (b) poly(S-alt-MIPOSS), (c) poly(AS-alt-MIPOSS), and (d) poly(HS-alt-MIPOSS) in CDCl3. |
![]() | ||
Fig. 3 29Si NMR spectra of (a) poly(MIPOSS), (b) poly(S-alt-MIPOSS), (c) poly(AS-alt-MIPOSS), and (d) poly(HS-alt-MIPOSS) in CDCl3. |
Fig. 4 displays the FTIR spectra of poly(MIPOSS), poly(S-alt-MIPOSS), poly(AS-alt-MIPOSS), and poly(HS-alt-MIPOSS) at room temperature. Characteristic absorption bands of the homopolymer and alternating copolymers appear at 2952–2874, 1781, 1709, and 1110 cm−1, representing isobutyl CH stretching, asymmetric imide CO stretching, symmetric imide C
O stretching, and Si–O–Si stretching in the maleimide isobutyl POSS structure. The spectrum of poly(HS-alt-MIPOSS) [Fig. 4(d)] features an absorption band at 3453 cm−1 for OH stretching; the signal at 1771 cm−1 for C
O stretching of the AS groups in Fig. 4(c) only decreased after deacetylation because it overlapped with the signal for asymmetric imide C
O stretching.
![]() | ||
Fig. 4 FTIR spectra of (a) poly(MIPOSS), (b) poly(S-alt-MIPOSS), (c) poly(AS-alt-MIPOSS), and (d) poly(HS-alt-MIPOSS) at room temperature. |
Fig. 5 displays FTIR spectra, in the range 1850–1650 cm−1, that reveal the presence of specific interactions in the alternating polymers. The spectrum of poly(MIPOSS) [Fig. 5(a)] features two characteristic absorption bands centered at 1781 and 1709 cm−1, corresponding to asymmetric imide CO and symmetric imide C
O stretching, respectively. These absorption bands shifted to lower frequencies for poly(S-alt-MIPOSS) [to 1774 and 1706 cm−1, respectively; Fig. 5(b)] and poly(AS-alt-MIPOSS) [to 1771 and 1705 cm−1, respectively; Fig. 5(c)]. More interestingly, the width at half-height decreased from 32.3 cm−1 for poly(MIPOSS) to 19.8 and 20.2 cm−1 for poly(S-alt-MIPOSS) and poly(AS-alt-MIPOSS), respectively, implying that the dipole–dipole interactions between the imide C
O groups of poly(MIPOSS) were disrupted and weakened upon insertion of the styrene and acetoxystyrene segments. The FTIR spectrum of poly(HS-alt-MIPOSS) [Fig. 4(d)] reveals that the signals of the C
O groups shifted to 1774 and 1704 cm−1, respectively, with a new signal appearing at 1688 cm−1, suggesting that hydrogen bonds existed between the C
O groups of the MIPOSS units and the phenolic OH groups of the HS units.45 Through curve-fitting with the Gaussian function, we calculated the area fraction of the hydrogen-bonded C
O groups of the MIPOSS units to be 39.3%.
![]() | ||
Fig. 5 FTIR spectra, in the range 1850–1650 cm−1, of (a) poly(MIPOSS), (b) poly(S-alt-MIPOSS), (c) poly(AS-alt-MIPOSS), and (d) poly(HS-alt-MIPOSS), recorded at room temperature. |
We recorded MALDI-TOF mass spectra to determine the molecular weights of our POSS-containing polymers and the sequence distributions of our alternating copolymers. It can be difficult to measure MALDI-TOF profiles of high-molecular-weight compounds because the mass resolution can be too weak to separate the individual chains.46–48Fig. 6 displays the MALDI-TOF mass spectrum of poly(MIPOSS), revealing that the molar mass of its individual chains could be determined. For example, the intense peaks m/z 2230.80, 3184.95, 4124.30, and 5065.17 correspond to two, three, four, and five units, respectively, of maleimide isobutyl POSS. The difference in the values of m/z between 2230.95 and 3184.30 is 954, equal to the molecular weight of the repeat unit of poly(MIPOSS). The difference in the values of m/z between 3184.95 and 4124.30 is not, however, equal to 954, probably because of the different chain ends after thermal fragmentation of AIBN after free radical polymerization.
Fig. 7 presents the mass spectrum of poly(S-alt-MIPOSS), where the intensities of the individual peaks are not exactly 100%, providing excellent evidence for its copolymer composition: perfectly alternating individual chains with equal numbers of styrene and MIPOSS units. By using MIPOSS as a monomer for free radical copolymerization, it became easy to distinguish the sequence distribution in the MALDI-TOF mass spectrum; because the molecular weight of MIPOSS is quite high (954 g mol−1), we could readily determine the number of units of MIPOSS in the poly(S-alt-MIPOSS) alternating copolymer. For example, the peak at m/z 4448.72 corresponds to four units of styrene and four units of MIPOSS, while that at m/z 5506.79 corresponds to five units of styrene and five units of MIPOSS, indicating that poly(S-alt-MIPOSS) had a perfectly alternating sequence of individual chains. The difference in the values of m/z between 4448.72 and 5506.79 is 1058 g mol−1, equal to the molecular weight of one styrene and one MIPOSS unit. The intense peak at m/z 4448.72 corresponds to four units of styrene (4 × 104.15 u), four units of MIPOSS (4 × 954 u), a chain end from AIBN, and a Ag ion (107.87 u); it is labeled 4:
4. The most intense peaks correspond to a perfectly alternating sequence, with ratios of styrene
:
MIPOSS of n − 1
:
n, n
:
n, and n + 1
:
n, such as 3
:
4, 4
:
4, and 5
:
4 (see the inset to Fig. 7). Only a few weak peaks correspond to the ratios of styrene
:
MIPOSS of n − 2
:
n and n + 2
:
n, such as 2
:
4 and 6
:
4, arising due to homopolymerization of styrene and MIPOSS; the fraction of such non-alternating segments was only 3.9%, based on the results of curve-fitting. Thus, MALDI-TOF mass spectral analysis suggested that we had obtained a near-perfect alternating copolymer of poly(S-alt-MIPOSS).
Interestingly, the mass spectrum of poly(AS-alt-MIPOSS) (Fig. 8) exhibited the same phenomenon as that of poly(S-alt-MIPOSS); for example, an intense peak at m/z 4761.6 (labeled 4:
4) corresponding to four units of 4-acetoxystyrene (4 × 162.19 u), four units of MIPOSS (4 × 954 u), a chain end from AIBN, and a Ag ion (107.87 u), as well as a peak at m/z 5879.3 (labeled 5
:
5) representing five units of MIPOSS and five units of 4-acetoxystyrene. The difference in the values of m/z between 4761.6 and 5879.3 is 1118 g mol−1, equal to the molecular weight of one 4-acetoxystyrene unit and one MIPOSS unit. Similarly, only a few weak peaks appeared corresponding to ratios of 4-acetoxystyrene
:
MIPOSS of n − 2
:
n and n + 2
:
n, such as 2
:
4 and 6
:
4, arising from homopolymerization of 4-acetoxystyrene and MIPOSS units, with the fraction of non-alternating segments being only 2.7% based on curve-fitting. This MALDI-TOF mass spectral analysis also implies that we had obtained a near-perfect alternating copolymer of poly(AS-alt-MIPOSS). The MALDI-TOF mass spectrum in Fig. 9 confirms that the chain of poly(HS-alt-MIPOSS) was also an alternating copolymer, with the intense peak at m/z 4478.6 (labeled 4
:
4) representing four units of 4-hydroxystyrene (4 × 120 u), four units of MIPOSS (4 × 954 u), a chain end from AIBN, and a Ag ion (107.87 u), as well as a signal at m/z 5552.3 (labeled 5
:
5) attributable to five units of MIPOSS and five units of 4-hydroxystyrene. The difference in the values of m/z between 4478.6 and 5552.3 is 1074 g mol−1, equal to the molecular weight of one 4-hydroxystyrene unit and one MIPOSS unit. The sequence distribution of poly(HS-alt-MIPOSS) should be the same as that of poly(AS-alt-MIPOSS), because we prepared it through deacetylation of the latter. Based on their MALDI-TOF mass spectra, our three copolymers appeared to be near-perfect alternating copolymers.
![]() | ||
Fig. 10 DSC thermograms of (a) poly(MIPOSS), (b) poly(S-alt-MIPOSS), (c) poly(AS-alt-MIPOSS), and (d) poly(HS-alt-MIPOSS). |
We recorded WAXD patterns (Fig. 11) of poly(MIPOSS), poly(S-alt-MIPSS), poly(AS-alt-MIPOSS), and poly(HS-alt-MIPOSS) at room temperature to examine their crystallinity. The WAXD profile of poly(MIPOSS) features four major diffraction peaks at 7.06 (101), 9.50 (110), 10.60 (102), and 16.43 (113) corresponding to the rhombohedral crystal structure of MIPOSS;49,50 accordingly, we observed a melting temperature, through DSC analyses, in Fig. 10. After alternative insertion of S, AS, and HS inert diluent segments into the MIPOSS segment, the WAXD patterns of poly(S-alt-MIPSS), poly(AS-alt-MIPOSS), and poly(HS-alt-MIPOSS) featured only broad peaks, with the crystalline peaks of poly(MIPOSS) disappearing; thus, these alternating copolymers had amorphous structures, consistent with DSC analyses in Fig. 10.
![]() | ||
Fig. 11 Wide-angle X-ray diffraction (WAXD) patterns of (a) poly(MIPOSS), (b) poly(S-alt-MIPOSS), (c) poly(AS-alt-MIPOSS) and (d) poly(HS-alt-MIPOSS) alternating copolymers. |
We performed TGA analyses under a N2 atmosphere (Fig. 12) to determine the decomposition temperatures (Td10 as the standard) and char yields of these alternating copolymers prepared through free radical copolymerization. The degradation temperature and char yield of poly(MIPOSS) (345 °C and 14.8%, respectively) were higher than those of PS (337 °C and 0%, respectively), consistent with the readier pyrolysis of the PS main chain from 300 to 450 °C.51,52 More interestingly, the value of Td10 and the char yield of poly(S-alt-MIPOSS) (397 °C and 9.5%, respectively) were higher than those of the standard PS as a result of the steric bulk of the rigid-cage MIPOSS units. In contrast, both the poly(AS-alt-MIPOSS) (376 °C and 28.1%, respectively) and poly(HS-alt-MIPOSS) (366 °C and 29.3%, respectively) alternating copolymers displayed relatively lower degradation temperatures and relatively higher char yields than those of poly(S-alt-MIPOSS) because, above their decomposition temperature, their acetyl and phenol moieties would tend to form aromatic char structures and increase the crosslinking densities of their organic/inorganic copolymers.50a
![]() | ||
Fig. 12 TGA profiles of PS, poly(MIPOSS), poly(S-alt-MIPOSS), poly(AS-alt-MIPOSS), and poly(HS-alt-MIPOSS), recorded under a N2 atmosphere. |
We used PL spectroscopy to investigate the emission properties of the homopolymer and the alternating copolymers in the solid state and the fluorescence behavior of poly(MIPOSS) and poly(S-alt-MIPOSS) at various concentrations (from 10−5 to 10−2 M) in THF with excitation at 330 nm. Fig. 13 presents the PL spectra of poly(MIPOSS), poly(S-alt-MIPOSS), poly(AS-alt-MIPOSS), and poly(HS-alt-MIPOSS) in the solid state. The intensities of the unexpected emissions of the oxygenic nonconjugated poly(MIPOSS) at 490 and 519 nm were higher than those of the alternating copolymers, presumably because of the clustering of the locked CO groups.15,16 On the other hand, poly(S-alt-MIPOSS), poly(AS-alt-MIPOSS), and poly(HS-alt-MIPOSS) exhibited fluorescence that resulted from pi–pi interactions between the phenyl rings and C
O groups in poly(MIPOSS). In addition, the emission intensities of the copolymers were lower than those of poly(MIPOSS), suggesting a lower degree of clustering of the locked C
O units of poly(MIPOSS) after alternative insertion of the styrene derivatives. Fig. S3† displays the photoluminescence spectra of poly(MIPOSS), poly(S-alt-MIPOSS), poly(AS-alt-MIPOSS), poly(HS-alt-MIPOSS) and poly(S-alt-MA) in THF solution (10−3 M). As shown in Fig. S3,† poly(MIPOSS) shows a strong emission peak at 496 nm, referring to its bulky anhydride group in the maleimide isobutyl unit, which hinders the free rotation of polymer chains along the C–C single bond.16bFig. 14 displays the effect of concentration on the emission behavior of poly(MIPOSS) and poly(S-alt-MIPOSS) in THF. The emission intensities of both poly(MIPOSS) and poly(S-alt-MIPOSS) increased upon increasing the concentration (from 10−5 to 10−2 M) in THF. In the most dilute solutions (10−5 M) of these oxygenic nonconjugated polymers, we observed no emissions because only a small amount of the luminogen was present.9c,12b,16,53,54 To examine the aggregation induced emission behavior of poly(MIPOSS) and poly(S-alt-MIPOSS), the effects of water content on photoluminescence spectra were determined in a THF/water mixture as predicted in Fig. S4.† Water is used here because it is a poor solvent for poly(MIPOSS) and poly(S-alt-MIPOSS), respectively. On increasing the water content from 0 to 80%, the corresponding solution in solution mixtures exhibited increased emission intensity due to the aggregation of luminogenic molecules with high water contents. The formation of a nanoaggregate structure has the role to activate the restriction of the intramolecular rotation (RIR) process. According to the concentration-enhanced emissions and the solvent pair effect in Fig. 14(A) and (B) and S4,† we suspect that poly(MIPOSS) and poly(S-alt-MIPOSS) may both be AIE materials. To confirm our hypothesis, we measured the quantum efficiencies (Φf) of poly(MIPOSS), poly(S-alt-MIPOSS), poly(AS-alt-MIPOSS), poly(HS-alt-MIPOSS), and poly(S-alt-MA) in the solid state, obtaining values of 72.5, 55.5, 46.8, 7.0, and 6.9%, respectively. Interestingly, the quantum efficiency of poly(S-alt-MIPOSS) was higher than that of poly(S-alt-MA), presumably because the POSS units were able to lock the C
O groups in the MIPOSS segments and, thereby, enhance the emission properties. In addition, the values of quantum efficiencies (Φf) of poly(MIPOSS), poly(S-alt-MIPOSS), poly(AS-alt-MIPOSS), poly(HS-alt-MIPOSS), and poly(S-alt-MA) in THF solution were 57.82, 5.52, 2.70, 5.64 and 1.72%, respectively. Dynamic light scattering (DLS) was measured to determine whether poly(MIPOSS) and poly(S-alt-MIPOSS) can form nanoaggregate structures in THF/H2O mixture solution as shown in Fig. S5.† The sizes of the particles of poly(MIPOSS) were 733, 580, 383, and 225 nm. While the sizes of particles of poly(S-alt-MIPOSS) were 906, 774, 728 and 586 nm on increasing the water content from 40 to 80% in the THF/water mixture media. The formation of shrunken aggregates of poly(MIPOSS) and poly(S-alt-MIPOSS) in solution on increasing the water volume fraction is responsible for the emission intensity enhancement in Fig. S4.†
![]() | ||
Fig. 14 Fluorescence spectra of (a) poly(MIPOSS) and (b) poly(S-alt-MIPOSS) as solutions in THF at concentrations from 10−5 to 10−2 M (excitation at 330 nm). |
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c5py01537e |
This journal is © The Royal Society of Chemistry 2016 |