Jin Won
Yu‡
ab,
Jin
Jung‡
a,
Yong-Mun
Choi
a,
Jae Hun
Choi
a,
Jaesang
Yu
a,
Jae Kwan
Lee
b,
Nam-Ho
You
a and
Munju
Goh
*a
aCarbon Composite Materials Research Center, Institute of Advanced Composites Materials, Korea Institute of Science and Technology (KIST), Chudong-ro 92, Bondong-eup, Wanju-gun, Jeollabuk-do 565-905, Korea. E-mail: goh@kist.re.kr; Tel: +82 63 2198141
bDepartment of Carbon Materials, Chosun University, Gwangju, 561-756, Korea
First published on 3rd November 2015
We synthesized diamine-functionalized graphene oxide, DDS–GO and HMDA–GO, by introducing 4,4′-diaminodiphenyl sulfone (DDS) or hexamethylenediamine (HMDA) into the carboxylic acid groups on graphene oxide (GO) via amide bonds. The introduction of diamines was confirmed by analytical methods such as FT-IR, TG-DTA, XPS, AFM, and optical microscopy. Then, we applied DDS–GO and HMDA–GO as co-curing agents for epoxy (EP) nanocomposites that were prepared by mixing bisphenol-A type EP and DDS curing agent (ca. 21 wt%). Interestingly, when 1.0 wt% of DDS–GO was added to the EP/DDS mixture, the crosslink density (CD) increased from 0.028 to 0.069 mol cm−3. Due to the higher CD, both the glass transition temperature and tensile strength of the EP/DDS/DDS–GO nanocomposite effectively improved from 160.7 °C to 183.4 °C and from 87.4 MPa to 110.3 MPa, respectively.
The use of carbon nanomaterials like carbon black,5 carbon nanotubes,6,7 carbon nanofibers,8 and graphene9–12 as fillers to prepare EP nanocomposites has been attracting attention owing to their unique properties. In addition to these nanomaterials, graphene oxide (GO) has been considered a promising nanomaterial for the improvement of the mechanical and thermal properties of polymer nanocomposites such as poly(methyl methacrylate), polystyrene, polyurethane, and poly(vinylidene fluoride) nanocomposites.13,14 Various neat and functionalized GOs have also been adapted for enhancing the glass transition temperature (Tg) and/or mechanical strength of EP nanocomposites.15–20 The crosslink density (CD) is generally recognized as a critical factor influencing the thermal21,22 and mechanical23,24 properties of EP nanocomposites. If the interfacial strength between the GO and EP is low, the CD of nanocomposites will be low, and because of the low CD value, improvements in the thermal and mechanical properties of EP nanocomposites cannot be sufficient and, in some cases, these properties can be worse. In order to improve the interfacial strength between GO and EP, some studies focused on the preparation of functionalized GOs with epoxide terminal groups15–17 and with amine terminal groups.18–20 In these studies, slight improvements in the Tg and tensile strength of cured EP nanocomposites compared to those of neat cured EPs were realized. Further, it has been mentioned that incorporation of nanomaterials into EP could slightly increase the CD of EP nanocomposites,25–30 but there have been few studies that calculated the CD of EP nanocomposites, made an effort to increase the CD of EP nanocomposites, and discussed the effect of the nanomaterials on the CD of EP nanocomposites.
In this work, we report a novel technique to improve the CD of GO-incorporated EP nanocomposites. We synthesized two diamine-functionalized GO, DDS–GO and HMDA–GO, by introducing 4,4′-diaminodiphenyl sulfone (DDS) or hexamethylenediamine (HMDA) into the carboxylic acid groups on GO via amide bonds. We prepared two kinds of mixtures, EP/DDS/DDS–GO and EP/DDS/HMDA–GO, by adding each diamine-functionalized GO as the co-curing agent into the mixture of diglycidyl ether of bisphenol-A (DGEBA)-type EP and 4,4′-diaminodiphenyl sulfone (DDS) curing agent (ca. 21 wt%). By increasing the amounts of DDS–GO from 0 to 1 wt%, the CD of EP/DDS/DDS–GO nanocomposites increased, and thus, we could effectively increase the Tg and tensile strength of EP nanocomposites.
![]() | (1) |
For example, the stoichiometric amount of DDS for 100 g of YD-128 was calculated to be 33 g. When diamine-GO was added in the nanocomposite, the mixing amount of the curing agent reduced to 80% of the stoichiometric amount of DDS, because the amine groups on DDS–GO could also react with epoxide groups as the curing agent. The content of diamine-GO was calculated based on the entire amount of the EP resin and curing agent. EP/DDS/diamine-GO nanocomposites were prepared with different weight fractions of the diamine-GO (0.1 wt%, 0.5 wt%, and 1 wt%). More details on the mixing ratios for obtaining EP nanocomposites are shown in the ESI (Table S1†). The fabrication procedure for EP nanocomposites is as follows. Stoichiometric amounts of diamine-GO and EP resin were mixed using a planetary mixer with the mixing speed of 2000 rpm for 10 min. After adding a stoichiometric amount of DDS to the mixture of EP/amine-GO, the mixture was further mixed by stirring at 155 °C for 20 min. Then, the mixture was placed in a vacuum to remove the trapped air bubbles and poured into a mold, followed by precuring it in an oven at 170 °C for 4 h and curing at 230 °C for 2 h.
![]() | ||
Fig. 2 (a) FT-IR spectra of GO, DDS, and DDS-GO. (b) TG-DTA curves of GO and DDS–GO during heating up to 900 °C under a N2 atmosphere. |
FT-IR analysis is an important technique to study the structural change in diamine-GO. Representative FT-IR spectra of DDS–GO are presented in Fig. 2a to provide the proof of the successful synthesis of DDS–GO. FT-IR spectra of HMDA–GO are given in the ESI (Fig. S1†). There are three characteristic absorption bands in the FT-IR spectra of DDS–GO. First, an absorption band at 3450 cm−1 attributed to the O–H stretching vibration derived from O–H groups on GO.33 This absorption band was quite broad, because the absorption band at about 3350 cm−1 assigned to the N–H vibration of the amine group on DDS34 combined with the O–H stretching vibration band of GO. Absorption bands corresponding to CC skeletal vibration at 1630 cm−1 and C
O stretching vibration in the spectra of GO33 and absorption bands of sulfone O
S
O stretching vibration at 1140–1325 cm−1 in the spectrum of DDS34 also appeared in the FT-IR spectrum of DDS–GO. Meanwhile, a strong absorption band newly appeared at 1647 cm−1 in the spectrum of DDS–GO. We assigned it to the stretching vibration of the amide group created by condensation of the carboxylic acid group at the GO edge with the amine group of DDS.19 These FT-IR analysis results are strong evidence of GO functionalization with the diamine derivatives.
Fig. 2b shows the TG-DTA curves of GO and DDS–GO under a N2 atmosphere (for the curves of HMDA–GO, see Fig. S2 in the ESI†). In the TG-DTA curve of GO, the small weight loss peak at 80 °C was due to the loss of residual water in GO, and the main weight loss peak that appeared around 210 °C is assigned to the pyrolysis of the labile oxygen functional groups, yielding CO, CO2, and steam.35,36 On the other hand, we could observe two different major loss peaks from the TG-DTA curve of DDS–GO. The peak near 160 °C could be ascribed to the loss of the remaining oxygen functional groups on GO, which slightly shifted to a temperature lower than that of non-functionalized GO. The peak around 270 °C corresponds to the decomposition of DDS.34 From the decomposed weight, we calculated the substituted amount of DDS in DDS–GO as 7 wt%. With this method, the substituted amount of HMDA in HMDA–GO was also evaluated as 7 wt%. The results of TG-DTA analysis also indicate that diamine derivatives were successfully introduced onto GOs.
Further investigation by XPS analysis was performed to characterize diamine-GOs, and the resulting deconvoluted XPS C 1s spectra of GO and DDS–GO are shown in Fig. 3 (for the spectra of HMDA–GO, see Fig. S3 in the ESI†). In Fig. 3a, five characteristic peaks were observed at 284.1, 285.5, 286.3, 287.8, and 290.0 eV, which correspond to C–C, C–OH, C–O–C, CO, and C(
O)–O, respectively. Further, an additional peak at 288.4 eV was observed, Fig. 3b, and it could be assigned to O
C–NH moieties.37 Integrated areas of the peaks corresponding to each chemical bond are listed in Table S2.† From the existence of the O
C–NH peak in the XPS results, we found that amide groups were newly formed in the functionalized GO.
![]() | ||
Fig. 3 XPS C 1s spectra of (a) GO and (b) DDS–GO. Deconvoluted curves represent the theoretical XPS spectra for different chemical bonds. |
Thus, the results of FT-IR, TG-DTA, and XPS analyses confirmed that diamine derivatives were successfully introduced onto GOs via amide chemical bonds.
AFM analysis was employed to study the morphologies of GO and diamine-GOs, and their images are shown in Fig. 4. From these images, the presence of the nanolayer-type GO is clearly observed. The width and thickness of GO and diamine-GO were determined by the analysis results. The image of GO showed 2.0 nm average thickness and 300–1100 nm width range. Further, images of DDS–GO and HMDA–GO revealed an average thickness of 1.0 nm and a width ranging from 100–500 nm. It is considered that the additional ultrasonication process in the case of the functionalized GO would shatter the GO into smaller pieces.
Good dispersion of nanomaterials greatly influences and improves the properties of the EP nanocomposites. Therefore, in order to investigate the dispersion state, EP/DDS/DDS–GO nanocomposites were observed by optical microscopy. The results are shown in Fig. 5, and they indicated that the DDS–GO dispersion in the EP nanocomposites was very homogeneous when the concentration was increased to 1.0 wt%. The presence of many polar moieties such as carboxylic acid, amide, and amine groups was thought to facilitate the dispersion of DDS–GO in the EP nanocomposite because they actively interact with EP via hydrogen or covalent bonding.
Addition of nanomaterials into the EP had a significant effect on the resulting thermal properties. As described in the Experimental section, diamine-GOs were used as co-curing agents of EP nanocomposites and their amount was controlled from 0.0 to 1.5 wt%. Curing temperatures were estimated from the temperatures of exothermic peaks in the first heating DSC curves of the EP/DDS/GO and EP/DDS/diamine-GO mixtures (for the DSC curves, see Fig. S4–6 in the ESI†), and are presented in Table S3.†Tg values of the cured EP/DDS/GO and EP/DDS/diamine-GO nanocomposites were determined based on endothermic peaks of their second heating DSC curves (Fig. 6, Table S4†) (for the DSC curves, see Fig. S7–9 in the the ESI†). When the GO was added to 1.0 wt% to the EP/DDS, the Tg of the EP/DDS/DDS–GO nanocomposite decreased from 160.7 to 136.8 °C. It has been reported that the non-functionalized GOs decrease the Tg of EP nanocomposites because of the tendency of GO to agglomerate in the polymer matrix and disturb the polymer heat flow, but this tendency has not been investigated sufficiently.38 In contrast, when 1.0 wt% of HMDA–GO or DDS–GO was added to the mixture of EP/DDS, the Tg of EP/DDS/diamine-GO nanocomposites remarkably increased to 170.5 or 183.4 °C, respectively; the high values obtained by adding HMDA–GO or DDS–GO are 125 and 135% which are higher than those for EP/DDS/GO nanocomposites, respectively. This is because the amine moieties functionalized on GO could improve the interfacial affinity by reacting with the epoxide groups of the EP resin. Subsequently, the disturbance of the interface between GO and EP could be reduced. If terminal amine groups on GO react with the epoxide groups of EP, diamine-GO could participate in the formation of a polymer crosslink network like the curing agent, and EP/DDS/diamine-GO nanocomposites would show higher CD than the EP/DDS/GO nanocomposite. Further, it is known that the CD of EP nanocomposites is closely related to their thermal properties.21,22
![]() | ||
Fig. 6 Glass transition temperatures (Tg) of EP/DDS/diamine-GO nanocomposites. Tg was estimated from the second heating DSC results of the EP/DDS/diamine-GO mixture. |
DMA measurements of EP/DDS/GO nanocomposites and EP/DDS/DDS–GO nanocomposites were performed to estimate the CD of EP nanocomposites. The storage modulus and tanδ of EP/DDS/DDS–GO nanocomposites are shown in Fig. 7a and b (for the DMA results of the EP/DDS/GO nanocomposite, see Fig. S10 in the ESI†). Based on the storage modulus and tan
δ in the rubber region, the CD of EP nanocomposites was calculated according to the following formula:30
![]() | (2) |
It has been also known that CD is not only related to the thermal properties of the EP nanocomposite, but also related to their mechanical properties.23,24 In order to investigate the effect of CD on the mechanical properties of the EP nanocomposite, the tensile strength of EP/DDS/diamine-GO nanocomposites was evaluated by UTM analysis; the analysis result is shown in Fig. 8 (for all results of UTM analysis, see Fig. S11–13 in the ESI†). Similar to the Tg, the tensile strength of the EP/DDS/DDS–GO nanocomposite was higher (110.3 MPa) than those of neat EP (87.4 MPa) and the EP/DDS/GO nanocomposite (74.3 MPa) when 0.1 wt% of DDS–GO or GO was added. When 0.1 wt% of HMDA–GO was added, the EP/DDS/HMDA–GO nanocomposite also showed higher tensile strength (90.4 MPa) than neat EP and the EP/DDS/GO nanocomposite, but the tensile strength is relatively smaller than the EP/DDS/DDS–GO nanocomposite (110.3 MPa) with 0.1 wt% of DDS–GO. In the EP/DDS/diamine-GO nanocomposites, diamine-GOs could have strong interactions with EP through covalent bonds between diamine-GOs and EP, and this is considered to be the reason for the improvement in the tensile strength of the EP/DDS/diamine-GO nanocomposite.
Meanwhile, both EP/DDS/HMDA–GO and EP/DDS/DDS–GO nanocomposites showed higher Tg and tensile strength values than the EP/DDS/GO nanocomposite, but the EP/DDS/DDS–GO nanocomposite exhibited superior properties to the EP/DDS/HMDA–GO nanocomposite. We thought that this result was due to the structural difference between HMDA, which has a flexible aliphatic structure, and DDS, which has a rigid aromatic sulfone structure. In the case of HMDA–GO, terminal amine groups are connected with GO through flexible alkyl chains, and these may cause a lower Tg and tensile strength of the EP/DDS/HMDA–GO nanocomposite than those of the EP/DDS/DDS–GO nanocomposite. In addition, terminal amine groups with different nucleophilicities exist. These terminal amine groups act as curing sites and are considered to be major factors that affect the thermal and mechanical properties of EP nanocomposites. HMDA has electron-rich aliphatic amine groups which can make the curing temperature of HMDA–GO lower than that of the main curing agent DDS. Consequently, a spatially heterogeneous curing reaction will take place in the nanocomposite, and this could negatively affect the thermal properties of EP/DDS/HMDA–GO. In contrast, DDS–GO starts to participate in curing at a similar temperature to DDS. Therefore, the curing reaction would occur more homogeneously in the EP/DDS/DDS–GO nanocomposite, and the thermal properties would be better. This hypothesis about the difference between HMDA–GO and DDS–GO was supported by the CD of EP/DDS/HMDA–GO, which was much lower than that of EP/DDS/DDS–GO. Moreover, the EP/DDS/DDS–GO nanocomposite showed increasing CD when more DDS–GO was added, while the CD of the EP/DDS/HMDA–GO nanocomposite did not change much despite the high contents of HMDA–GO.
Footnotes |
† Electronic supplementary information (ESI) available: Results of FT-IR spectra, TD-TGA curves, XPS spectra, DSC curves, DMA analysis, and UTM analysis of EP nanocomposites. See DOI: 10.1039/c5py01483b |
‡ These authors contributed equally. |