Juan Diego
Rodriguez-Blanco
*,
Samuel
Shaw
and
Liane G.
Benning
School of Earth and Environment, University of Leeds, Leeds, LS2 9JT, United Kingdom. E-mail: j.d.rodriguez@see.leeds.ac.uk
First published on 10th November 2010
The kinetics and mechanisms of nanoparticulate amorphous calcium carbonate (ACC) crystallization to calcite, viavaterite, were studied at a range of environmentally relevant temperatures (7.5–25 °C) using synchrotron-based in situ time-resolved Energy Dispersive X-ray Diffraction (ED-XRD) in conjunction with high-resolution electron microscopy, ex situX-ray diffraction and infrared spectroscopy. The crystallization process occurs in two stages; firstly, the particles of ACC rapidly dehydrate and crystallize to form individual particles of vaterite; secondly, the vaterite transforms to calcitevia a dissolution and reprecipitation mechanism with the reaction rate controlled by the surface area of calcite. The second stage of the reaction is approximately 10 times slower than the first. Activation energies of calcite nucleation and crystallization are 73 ± 10 and 66 ± 2 kJ mol−1, respectively. A model to calculate the degree of calcite crystallization from ACC at environmentally relevant temperatures (7.5–40 °C) is also presented.
Recent studies have shown that the chemical composition of ACC is nominally CaCO3·H2O.7 The ACC structure consists of a calcium-rich nanoscale framework with pores containing water and carbonate ions. The pores are approximately 1 nm in diameter and interconnect to form channels which run through the particles of ACC. ACC is thermodynamically unstable, and will spontaneously crystallize when suspended in an aqueous solution at ambient temperatures. This process is rapid (minutes to hours) and leads to the formation of calcite, aragonite and/or vaterite depending on the physical and chemical conditions. Pure ACC (non-additives) will transform to calcitevia a vaterite intermediate at low temperatures (<30 °C) and to aragoniteviavaterite at higher temperatures (≥40 °C).8,9 Impurities substituted into ACC can also influence the crystallisation pathway, with the addition of magnesium leading to the crystallisation of calcite, with no vaterite intermediate.9–11 Ogino et al. (1987)9 used measurements of solution chemistry and X-ray diffraction to characterize the pure ACC formation and transformation. Their data indicate that the initial ACC precipitated rapidly and transformed to vaterite within minutes. The vaterite in turn transformed to calcitevia a dissolution-reprecipitation mechanism. Kinetic studies of this second crystallization step at elevated temperatures (25–80 °C) using mixtures of vaterite and calcite seeds12 suggested that calcite growth was the rate determining step.
Currently, there is a lack of kinetic and mechanistic information on the crystallization of ACC at temperatures equivalent to those where biomineralization occurs in the natural environment (<25 °C). This is primarily because no study has systematically analyzed the complete transformation from precipitation of ACC to calcite, viavaterite. Furthermore, most studies have only characterized individual components of this crystallization reaction (e.g.vaterite to calcite12) and were performed using ex situ analyses with relatively low temporal resolutions (from 10's of minutes to 10's of hours). In this study we have used in situsynchrotron-based Energy Dispersive X-ray diffraction (ED-XRD) at a high temporal resolution (<1 min) in conjunction with high-resolution electron microscopy and infrared spectroscopy to characterize ACC formation and its crystallisation to calcite, viavaterite. This data provides a detailed mechanistic insight into the transformation mechanisms of both ACC to vaterite and vaterite to calcite. Also, the time-resolved diffraction data has been used to derive a model for the formation of calcite from ACC at temperatures relevant to biomineralization and industrial synthesis processes.
Experiments analogous to those performed on-line were undertaken off-line in order to obtain samples for solid characterization at various time intervals during the crystallization reaction. The solids precipitated immediately after mixing were quenched by vacuum-filtration (0.2 μm polycarbonate filters) and washed with isopropanol following the procedure described in Rodriguez-Blanco et al. (2008).16 The remaining solid phases (>30 s after mixing, i.e. intermediate phases and end-products) were separated from the aqueous solutions by centrifugation and filtration after which they were washed with isopropanol and dried at 25 °C in an oven. All off-line solids were characterized with a Bruker D8 powder X-ray diffractometer with a Ge(111) monochromator, (Cu-Kα1 = 1.54 Å; 2θ = 5–70° range; patterns recorded at 0.001° steps at 0.5 s/step) for their mineralogical composition. XRD patterns of the poorly ordered samples obtained immediately after mixing (1–30 s) were recorded at a slower scan rate (2 s/step) in order to improve the clarity of the low intensity diffraction peaks.
Fourier transform infrared spectra (FTIR) were acquired over the mid infrared region (650 to 4000 cm−1) using an A2-Technology MicroLab Portable mid-IR spectrometer, with a diamond internal reflection (DATR). Spectra were accumulated by co-adding 512 scans with a 4 cm−1 resolution and spectral manipulation including baseline adjustment, smoothing, normalization, and band component analysis was carried out using the Thermo Nicolet OMNIC ESP 5.1 software package. High resolution images of the solids were acquired using a Field Emission Gun Scanning Electron Microscope (FEG-SEM, LEO 1530 Gemini at 3KeV).
Finally, the saturation indexes (SI) for the different solid phases and their Ion Activity Products (IAP) were calculated with the geochemical code PHREEQC, using the initial solution composition and the solubility products for ACC17 and CaCO3 polymorphs18 as integrated in the wateq4f database.19
Fig. 1 (a) Three-dimensional representation of time-resolved ED-XRD patterns showing the evolution of vaterite (101), (102) and calcite (104) and (110) reflections at 7.5 °C. Energy has been converted to 2θ using the Bragg equation (2dsinθ = nλ) and assuming λ = 1.541 Å for Cu-Kα. (b) X-ray diffraction patterns of solids collected at different elapsed times during the off-line experiments, showing ACC, vaterite and calcite solid phases. |
Immediately upon mixing the starting solutions, a gel-like white precipitate formed. This initial precipitate exhibited no distinct diffraction peaks in the ED-XRD patterns and revealed only a broad hump derived from the combined scattering from the poorly-ordered precipitate and the aqueous solution. The off-line XRD patterns (pattern A in Fig. 1b) confirmed that this initial precipitate consisted of a poorly-ordered material, with two broad humps at approximately 30° and 45° 2θ which are characteristic of ACC.16FTIR spectra of this initial phase (Fig. 2, bottom pattern) were characterized by a broad band between 2700 and 3600 cm−1 (O–H stretching) and a shaper band at 1650 cm−1 (O–H bending), both of which correspond to structural water within ACC (water contents can reach up to 18wt%).20 In addition, ACC was also confirmed by the presence of a shoulder on the main asymmetric ν3CO3 band (at 1460 cm−1)21 and the absence of the ν4 symmetric vibration at 725 cm−1. This latter vibration is characteristic of crystalline calcium carbonate phases only (upper pattern in Fig. 2). The remaining bands representing the vibrations of the carbonate ions (1805, 1409, 1090 and 874 cm−1)22 are common in both poorly-ordered ACC and crystalline polymorphs.
Fig. 2 Fourier Transform Infrared (FTIR) spectra of ACC and calcite showing the change in water content from the amorphous hydrated precursor and the non-hydrated crystalline calcium carbonate phases. ‘A’ and ‘F’ represent the same samples shown in the XRD patterns (Fig. 1). |
As the reaction progressed the ED-XRD patterns revealed that the broad hump started decreasing and after a temperature-dependent induction time the vaterite (101) and (102) peaks started growing (Fig. 1a). These peaks rapidly increased in intensity as vaterite crystallized until they reached a maximum (e.g., at 7.5 °C after ∼1 h; see Fig. 3). Once a maximum was reached the vaterite peak intensities started to decrease and this was mirrored by the growth of the calcite (104) and (110) peaks. Calcite was the sole crystalline phase at the end of all experiments. This crystallization pathway was observed in all experiments and in all cases the crystallization reaction followed a two-stage process. In a first stage, the initially precipitated ACC crystallized to the intermediate calcium carbonate polymorph vaterite. The second stage of the transformation reaction was controlled by the crystallization of vaterite to calcite. The relative time length of the two-stage crystallization pathway is clearly observed when the changes in the degree of reaction for vaterite and calcite for an experiment are presented as a function of time (e.g. 7.5 °C, Fig. 3).
Fig. 3 Degree of reaction (α) determined from the dissolution of vaterite (101) and growth of calcite (104) reflections as a function of time at 7.5 °C. The ACC-vaterite and vaterite-calcite transformations are differentiated as stages 1 and 2, respectively. |
SEM photomicrographs of the solids from stage 1 (Fig. 4a–e) revealed that the ACC obtained immediately after mixing consisted of nanoparticles <50 nm in diameter with roughly spherical shape and low polydispersity (Fig. 4-a). The vaterite, which crystallized after ACC, formed large aggregates (<500 nm, Fig. 4-b). These vaterite aggregates consisted of nanoparticles with similar dimensions to the nanoparticulate ACC (Fig. 4-c). These vaterite spheres coexisted for a brief period (<15 min at 7.5 °C) with the precursor ACC nanoparticles. As the reaction progressed, the poorly-ordered ACC fully disappeared and only the micron-sized vaterite aggregates remained (Fig. 4-d,e). In stage 2, as the crystallization progressed the amount of vaterite decreased and calcite crystals formed on the surface of the vaterite aggregates (Fig. 4f-g, corresponding to XRD patterns D and E in Fig. 1b). During the final stages of calcite growth, the amount of vaterite progressively decreased until only individual nanoparticulate subunits (<50 nm) (Fig. 4-h) were present on the surface of the newly formed calcite crystals. The final end product, calcite, consisted of euhedral and subhedral crystals, which frequently showed pseudospherical casts after vaterite (Fig. 4-i). These casts were a product of the calcite forming on and around the spherical aggregates of vaterite.
Fig. 4 FEG-SEM images of the solid phases which form during the two stages of the crystallization experiments. Pictures on the top correspond to Stage 1, showing amorphous calcium carbonate (ACC, a); ACC and vaterite nanoaggregates (b, c); and vaterite nanoaggregates (d, e). Pictures at the bottom correspond to Stage 2: vaterite nanoaggregates and first calcite crystals (f); calcite crystals attached to vaterite spheres with the development of growth steps on the calcite surface (g); calcite growth steps and vaterite nanoparticulate subunits (h) and calcite crystals with vaterite casts (i). |
Fig. 5 Degree of reaction (α) determined from the vaterite (101) peak area and from the ED-XRD background intensity at 7.5 °C. Characters A to D represent the samples taken from the off-line experiments after specific elapsed times which are also correlated with XRD (Fig. 1b) and FTIR (Fig. 2). |
Combining information from the diffraction, electron microscopy and infrared spectroscopy, the key structural and physical processes which control the ACC to vaterite crystallization can be derived; firstly, the SEM images show that vaterite consists of aggregated nanoparticle sub-units which were smaller in average size (∼30 to 70 nm) than the primary ACC particles (∼20 to 45 nm) (Fig. 4). Secondly, the loss of the water as revealed by FTIR indicates that ACC dehydrated during its transformation into crystalline CaCO3 (Fig. 2). Thus, we infer that the transformation of ACC to vaterite is due to the rapid dehydration of the ACC structure followed by an internal structural reorganisation within the individual nanoparticles to form vaterite. The reduction of the XRD background intensity prior to the formation of vaterite may be due to initial dehydration and local ordering of the ACC structure prior to the formation of crystalline vaterite. This crystallization mechanism is supported by the recent work of Goodwin et al. (2010),7 who suggested that the local coordination environment of Ca in the nanoframework structure of ACC is similar to those in crystalline CaCO3 phases (e.g.vaterite and calcite). Therefore the dehydration and condensation of the ACC structure could lead to the formation of vaterite without major structural rearrangements. This mechanism is supported by the small change in particle size, which suggests that the individual ACC nanoparticles have indeed transformed to vaterite. Furthermore, the lack of defined crystal faces on the vaterite sub-units (Fig. 4-d) suggests they have not formed by controlled precipitation from solution, which usually leads to particles with a defined crystalline morphology. All these lines of evidence and observations suggest that the formation of vaterite is controlled by the breakdown of ACC and that this transformation occurs via a progressive dehydration of the ACC combined with aggregation and crystallization of ACC to form vaterite.
The changes in vaterite and calcite diffraction peak areas at all temperatures evaluated here during stage 2 are presented in Fig. 6 and 7. The data show that the rate of both the vaterite breakdown and calcite growth increase with time. Ogino et al. (1990)12 suggested, in seeded experiments, that the transformation of vaterite to calcite was dependent of the surface area of calcite present. In the current study, as the reaction progresses the amount of newly formed calcite surface also increases and thus the rate of reaction increases as the transformation occurs. This indicates that the vaterite dissolves releasing calcium and carbonate into solution, which then reprecipitate on the surface of the growing calcite crystals. This mechanism is supported by the SEM observations (Fig. 4), which clearly show the calcite crystals growing on the surface of the vaterite aggregates. In addition, the spherical casts still evident in the final calcite crystals (Fig. 4-i) suggest that the dissolution of vaterite and the precipitation of calcite are separate processes, further supporting the hypothesis that the transformation of vaterite to calcite is not a solid-state transformation but a surface-controlled process.
Fig. 6 Degree of reaction (α) determined from the dissolution of vaterite (101) reflection as a function of time at four different temperatures (7.5 to 25 °C). |
Fig. 7 Degree of reaction (α) determined from the growth of calcite (104) reflection as a function of time at four different temperatures (7.5 to 25 °C). The fitting curves using eqn (1) from Ogino et al., (1990)12 kinetic model are also shown as solid lines for all the plots. |
The calcite diffraction peak area growth as a function of time was fitted using the kinetic model developed by Ogino et al. (1990),12 which has been used to define the formation of calcite from vaterite in seeded systems:
α = (b(t − t0) + c)3 | (1) |
(2) |
fx = [(IAP)½ − (Ksp)½] | (3) |
The kinetic model (1) was fitted to the diffraction data for calcite formation at 25 °C to derive values for b and c (Table 1). A0 was taken to be the value of α at t0 (i.e. when vaterite starts to breakdown). s0 could then be calculated by substituting the rate constant for calcite formation at 25 °C (2.67 × 102s−1) from Ogino et al. (1990)12 into eqn (2), which produced a value of 0.188 m2. If it is assumed that the density of calcite is 2.71g cm−3 and that the crystals of calcite are rhombohedral in shape, which was confirmed by the SEM images (Fig. 4), the particle size of calcite at t0 can be calculated to be 0.63 μm. This estimate is consistent with the SEM images of the initial calcite crystal size formed during the transformation which are between 0.5 and 1 μm (Fig. 4-f). This particle size was then used to calculate s0 at all temperatures using the measured values of A0, assuming rhombohedral particle shape and the density of calcite. Following this the rate constant for calcite growth (k) was calculated at each temperature.
Calcite crystallization | |||||
---|---|---|---|---|---|
T/°C | Induction time/s | k (·102 s−1)(this study) | k (·102s−1)12 | b (·10−6) | c |
a Data has been fixed to match with Ogino et al. (1990) in order to calculate the initial particle size of calcite. | |||||
7.5 | 5100 | 0.71(0) | 2.10(1) | 0.0805(5) | |
10 | 2880 | 0.86(0) | 3.52(1) | 0.1013(4) | |
20 | 936 | 2.19(0) | 7.18(2) | 0.0719(4) | |
25 | 792 | 2.67a | 2.67 | 7.66(4) | 0.0724(5) |
30 | 4.67 | ||||
40 | 11.0 | ||||
50 | 28.3 | ||||
60 | 58.3 | ||||
Ea(nucl) (KJ/mol) | 73(10) | ||||
lnA(nucl) (s−1) | 23(4) | ||||
Ea(cryst) (KJ/mol) | 66(2) | ||||
lnA(cryst) (s−1) | 32(1) |
Rate constants (k), induction times (t0) and the b and c parameters for the growth of calcite at all temperatures are shown in Table 1. The derived induction times and rate constants as a function of temperature were used to calculate apparent activation energies for nucleation (Ea(nucl.)) and crystallization (Ea(cryst.)) for calcite using an Arrhenius approach13 (Table 1 and Fig. 8). The data on the Arrhenius plot describing calcite growth shows an excellent linear correlation (R2 >0.99) between the rates from this study and those from Ogino et al. (1990),12 indicating that the data from these two studies can be combined. The derived Ea(cryst.) value for calcite growth using the data from both studies is 66 ± 2 kJ mol−1. This activation energy for calcite formation is within the range suggested for surface-controlled reactions (<34 kJ mol−1).24 Also, several other authors have derived activation energies for seeded calcite growth ranging from ∼39 to ∼70 kJ mol−1,25–28 which are similar to the value derived in this study.
Fig. 8 Arrhenius plots for calcite nucleation (top) and crystallization (bottom). Kinetic data from Ogino et al. (1990)12 is included in the latter. |
An equation to model the degree of calcite crystallization from ACC at any given temperature can be derived by the rearrangement of eqn (1) and incorporating the rearranged Arrhenius equation for induction time (t0) as a function of temperature. This produces a model for the degree of calcite formation (α) as a function of time at a range of temperatures:
(4) |
This journal is © The Royal Society of Chemistry 2011 |