Langlang
Qin
a,
Yunfei
Gao
*b,
Caiyun
Han
a,
Minghui
Zhu
d and
Shuang
Wang
*ac
aCollege of Environmental Science and Engineering, Taiyuan University of Technology, Jinzhong 030600, Shanxi, P. R. China. E-mail: wangshuang@tyut.edu.cn
bInstitute of Clean Coal Technology, East China University of Science and Technology, Shanghai 200237, P. R. China. E-mail: yunfeigao@ecust.edu.cn
cShanxi Key Laboratory of Gas Energy Efficient and Clean Utilization, Taiyuan University of Technology, Taiyuan 030024, Shanxi, P. R. China
dState Key Laboratory of Chemical Engineering, School of Chemical Engineering, East China University of Science and Technology, Shanghai 200237, PR China
First published on 4th July 2024
The hydrogenation of carbon dioxide (CO2) to methanol is an important reaction to convert CO2 into valuable products and reduce carbon emission. MoS2 is an effective catalyst for CO2 hydrogenation, but the synergistic effects of interlayer spacing expansion and surface sulfur vacancy strengthening have not been studied systematically. Here, this work reports hydrazine hydrate as an effective reducing agent for MoS2. The reducing agent can not only expand the interlayer spacing of MoS2, but also increase the concentration of sulfur vacancies through a simple treatment. More importantly, the synergistic effect between the interlayer spacing and sulfur vacancies of MoS2 significantly increases the methanol space-time yield (STY). At 220 °C, 4 MPa, and 8000 mL gcat−1 h−1, the MoS2–N2H4-4 catalyst exhibits 76.8% methanol selectively, 5.52% CO2 conversion, and a high methanol STY of up to 0.1214 g gcat−1 h−1 and lasts for at least 200 h. The structure–performance relationship was further studied using physio-chemical characterization and DFT. These results provide valuable insights into the development of highly efficient MoS2 catalysts for CO2 hydrogenation.
In recent years, molybdenum disulfide (MoS2) has been explored in the process of CO2 hydrogenation to methanol and has shown excellent performance.12–15 There is a strong structure–activity relationship between the morphology of MoS2 and its CO2 hydrogenation performance.16,17 For example, Deng et al. prepared few-layer MoS2, which achieved a selectivity of 94.3% for methanol and a conversion of 12.5% of CO2 at 180 °C, attributed to the exposure of more active sites in the few-layer structure.18 Zhou et al. developed boxlike assemblies of quasi-single-layer MoS2 nanosheets (h-MoS2/ZnS), and the space-time yield (STY) of CO2 hydrogenation to methanol reached 0.93 gCH3OH gMoS2−1 h−1 at 260 °C.19 More importantly, highly dispersed molybdenum disulfide nanosheets with fewer layers can promote the generation of abundant active sites. They discovered that CO2 is decomposed into CO* on MoS2, leading to improved selectivity of methanol.18,19 In addition to the few-layer structure of MoS2, sulfur vacancies also play a key role in its catalytic ability. Fei et al. found that the presence of Sv caused an upshift in the d-band centre according to density functional theory (DFT), which enhanced the adsorption of reaction intermediates.20 They prepared a FL-MoS2-20 catalyst with a Sv concentration of 16.3% by a chemical reduction method, which showed excellent NH3 yield. Zhou et al. pointed out that the appropriate Sv concentration of MoS2 can greatly improve its proton adsorption/desorption capacity.21 From theoretical and experimental results, it can be seen that strengthening Sv while maintaining the few-layer structure has the potential to achieve the enhancement of catalytic performance.
The current techniques for Sv construction primarily include plasma treatment,22–25 heteroatom doping,14,17,26–28 chemical reduction,21,29–31etc., enabling precise control over the concentration of Sv. Jin et al. synthesized a NiS2 catalyst by using an argon plasma etching strategy; when the concentration of Sv was 5.9%, its hydrogen evolution reaction (HER) performance was greatly improved.32 Zhou et al. used hydrothermal doping of copper into MoS2 nanosheets, which doubled the number of Sv on MoS2, thereby increasing the STY of CO2 hydrogenation to methanol by 2.27 times.33 However, ion etching and heteroatom doping are relatively complex, and Ma et al. constructed a MoS2/C composite with Sv by chemical reduction, and used hydrazine hydrate to regulate the concentration of Sv to achieve efficient storage of Na+.34 The chemical reduction method is used to post-treat the catalyst, which is easy to operate and can accurately regulate Sv. Hence, the chemical reduction method is a simple and effective strategy for constructing Sv.
In this work, a series of MoS2 catalysts with different Sv concentrations and interlayer spacing were prepared by the chemical reduction method, and the Sv concentration in MoS2 was regulated by changing the concentration of hydrazine hydrate. By comparing different reductants, it was found that the MoS2–N2H4-4 catalyst had abundant Sv and large interlayer spacing. The characterization results showed that hydrazine hydrate successfully regulated both the concentration of Sv and interlayer spacing. Theoretical calculations show that the introduction of Sv can increase the electron density of Mo atoms, enhance the adsorption capacity of MoS2 to CO2, and increase the methanol STY. The synergistic effect of interlayer spacing and Sv plays a momentous role in tuning the activity of MoS2.
The composition of the sample was analyzed by X-ray diffraction (XRD) and the resulting XRD data were compared with the standard spectra of 2H-MoS2. As shown in Fig. 1b and S1,† all diffraction peaks were observed to coincide with those of 2H-MoS2, indicating that the MoS2 phase was successfully prepared in the sample. Upon chemical reduction, the XRD spectra of all samples revealed diffraction peaks characteristic of MoS2, which were observed to be consistent with the peak positions documented in PDF-37-1492. Specifically, the diffraction peaks at approximately 33.5° and 58.3° corresponded to the (100) and (110) planes, respectively, while the most prominent peak of the (002) plane was located at 14.3°. Observably, the peak intensity of the (002) crystal plane decreased for all three catalysts, and the peak intensity of MoS2–NH3 was the lowest, which was theoretically attributed to the monolayer or the few-layer structure of MoS2.35 Interestingly, with the increase of hydrazine hydrate addition, the (002) reflection peak of MoS2–N2H4-8 appeared to be almost unidentifiable, indicating the stacking of only a few MoS2 layers in the c-direction. Furthermore, no additional peaks were observed after chemical reduction treatment, demonstrating that the chemical reduction reaction utilizing reductants did not produce other phases or alter the crystal structure.
N2 adsorption/desorption experiments were carried out at 77 K to investigate the pore properties and specific surface area of the prepared catalyst. As shown in Fig. 1c and S2,† N2 physisorption isotherms indicated that these samples all exhibit typical type-IV curves and a distinct H3-type hysteresis loop, a distinctive characteristic of mesoporous materials. The Brunauer–Emmett–Teller (BET) specific surface areas of MoS2, MoS2–N2H4-4, MoS2–NH3 and MoS2–NaBH4 were determined to be 16.1, 26.1, 37.5 and 26.5 m2 g−1 (Table S1†), respectively, indicating an increased specific surface area after chemical treatment.
To determine whether the reduction by the three reductants has disrupted the original morphology, all the samples were observed under an electron microscope (SEM) (Fig. 2a1–d1 and S3†). Overall, all the samples were spherical in shape, composed of tiny nanosheets forming a nanoflower morphology, with particle diameters ranging from 300 nm to 500 nm, and their appearance remained unchanged following the chemical reduction reaction with hydrazine hydrate. The well-defined structure with a nanoflower was further confirmed by the TEM technique (Fig. 2a2–d2). Moreover, the sample exhibits stacked spheres with a diameter of approximately 300–350 nm. There were many transparent layers in the nanoflower of MoS2–N2H4-4 and MoS2–NH3, which confirmed that the two catalysts had fewer layers, consistent with the results of XRD analysis. In addition, the high-resolution transmission electron microscopy (HRTEM) images (Fig. 2a3–d3) showed a typical lamellar structure with a well-resolved d-spacing. It can be clearly seen that the original MoS2 nanoflower has more edges that exhibit a layer-to-layer spacing value of 0.64 nm, which is consistent with the XRD results. Besides, there are lattice fringes observed in the MoS2–N2H4-4 and MoS2–NH3 nanostructures that correspond to the (002) plane of MoS2 with an enlarged interlayer spacing of 0.74 nm. This is because the intercalation of ammonium expands the interlayer spacing of MoS2 during synthesis, thus favoring the exposure of more active sites.36,37 In contrast, sodium borohydride has a lower reducing ability. The layer spacing does not change and remained at 0.64 nm.
Fig. 2 (a1–d1) SEM, (a2–d2) TEM and (a3–d3) HRTEM images of (a1–a3) MoS2, (b1–b3) MoS2–N2H4-4, (c1–c3) MoS2–NH3 and (d1–d3) MoS2–NaBH4 catalysts. |
The d(002) of MoS2 was analyzed and measured using Bragg's law (2dsinθ = nλ) for XRD data (Fig. 1b and S4†). The calculation results (Table S1†) show that the d(002) of MoS2–N2H4-4 is close to that of MoS2–NH3 and larger than that of MoS2 and MoS2–NaBH4, which is consistent with the TEM test results.
It was validated that Sv concentration can be further increased by chemical reduction treatment with hydrazine hydrate. According to Fig. 3b and S6a,† it can be found that with the increase of the dosage of hydrazine hydrate, the characteristic Mo peak moves towards lower binding energy and the Moδ+ peak area increases, which may be due to the reduction of hydrazine hydrate. In the S 2p XPS spectra of all the samples (Fig. 3c), the two peaks of S 2p3/2 and S 2p1/2 at 162.2 and 163.4 eV can be clearly distinguished in MoS2. Compared with the S 2p XPS spectra of MoS2, MoS2–N2H4-4 and MoS2–NaBH4 sample characteristic peak shift occurs, and this may be related to the generation of Sv.40 In contrast, ammonia liquor can only expand the interlayer spacing, and the two peaks of S 2p did not change. In addition, significant peak shifts were also observed in the S 2p XPS spectra of MoS2–N2H4-2 and MoS2–N2H4-8 (Fig. S6b†). With the increase of hydrazine hydrate addition, the peak shift was more obvious, indicating the presence of more Sv.41,42
The structural characteristics of Sv in these catalysts were investigated by Raman spectroscopy in this experiment. As shown in Fig. 3d, all samples exhibited the main characteristic Raman vibration peaks of MoS2 at 360–420 cm−1, corresponding to the in-plane Mo–S phonon mode (E12g) and out-of-plane Mo–S mode (A1g), respectively.43,44 The A1g and E12g vibration modes have changed for the expanded interlayer MoS2 materials as compared to MoS2.45 In detail, the A1g peaks blue shift from 408.2 cm−1 for MoS2 to 404.4 cm−1 for MoS2–N2H4-4 and to 406 cm−1 for MoS2–NH3 and to 405.4 cm−1 for MoS2–NaBH4, while the E12g peaks shift from 376 cm−1 for MoS2 to 378.2 cm−1 for MoS2–N2H4-4 and to 375 cm−1 for MoS2–NH3 and to 373 cm−1 for MoS2–NaBH4. It was worth noting that the E12g and A1g peak spread of MoS2–N2H4-4 and MoS2–NaBH4 was wider than that of MoS2. This is due to the Sv perturbation in the 2H lattice resulting in the reduction of the Mo–S bond and the weakening of the energy of the vibration mode, resulting in the melting of the Mo–S phonon mode in the principal plane.46–48 The above results are in agreement with our results using the XPS method. In addition, the distance between the E12g and A1g peaks of MoS2–N2H4-4 and MoS2–NH3 was reduced, indicating a diminished interaction between adjacent MoS2 layers, because the interlayer spacing of MoS2–N2H4-4 and MoS2–NH3 was expanded compared to the original MoS2. MoS2–N2H4-2 and MoS2–N2H4-8 also conform to the above rules (Fig. S7†); with the increase of the amount of hydrazine hydrate, the peak position is shifted, and the peak spread becomes wider, indicating that the Sv concentration increases (Table 1).49
In order to visually demonstrate the concentration changes of Sv in catalysts, MoS2, MoS2–N2H4, MoS2–NH3, and MoS2–NaBH4 were characterized by electron paramagnetic resonance (EPR).50–53 The signal at ∼330 mT (g = 2.0) in Fig. S8† indicated the concentration of unsaturated sites with unpaired electrons, which is proportional to the Sv in the sample. The analysis of the data revealed that original MoS2 exhibited some EPR signals, indicating that the MoS2 catalyst can generate some Sv after H2 activation. MoS2–NaBH4 exhibited the highest EPR signal, suggesting the strongest charge compensation effect and thus the highest Sv concentration. However, this contradicts the significant increase in methanol production with increasing Sv. This phenomenon is attributed to the change in the nature of the defects. Under the appropriate reducing agent's reduction ability, “point” defects are formed. Excessive reduction ability causes S atoms to detach, resulting in larger defects,54,55 and exposed edge S vacancies are not conducive to methanol production. Additionally, the peak area and intensity of MoS2–N2H4 were significantly higher than those of MoS2 and MoS2–NH3, indicating that MoS2 expands the interlayer spacing while undergoing reduction, leading to more sulfur vacancies. Therefore, both the reducing ability of the reducing agent and the enlargement of the interlayer distance contribute to increasing the number of Sv. Combining TEM, XPS and EPR test results, it is found that the enriched Sv may also contribute to the enlarged interlayer spacing.
To summarize, N2H4·H2O, NH3·H2O and NaBH4 treatments all lead to changes in the original MoS2 in terms of the structure, morphology and sulfur vacancies. But the effects are different due to their distinct chemical reduction and interlayer expansion capabilities. In short, NaBH4 can lead to the enhancement of sulfur vacancies but did not expand the interlayer spacing substantially. NH3·H2O expands the interlayer spacing but did not lead to the enhancement of sulfur vacancies due to its lack of reducing capabilities. Meanwhile, N2H4·H2O leads to both enhanced sulfur vacancies and increased interlayer spacing. The effects of these structure, morphology and sulfur vacancy changes will be elaborated in the following section.
According to the above performance comparison, it is found that hydrazine hydrate treated MoS2 has the best performance. Therefore, the added amount of hydrazine hydrate was optimized, and the optimized results are shown in Fig. S9 and S10.† Under the conditions of 4 MPa, 220 °C and GHSV = 8000 mL gcat−1 h−1, the methanol STY initially increased with the increase of the addition of hydrazine hydrate, and when the addition of hydrazine hydrate reached a certain amount (4 mL), the performance of the catalyst was stable and no longer increased, which indicated that the performance of the catalyst may be limited by other factors. After analysis, it was found that MoS2–N2H4-2, MoS2–N2H4-2 and MoS2–N2H4-8 had similar product selectivity, but MoS2–N2H4-2 had lower CO2 conversion, resulting in lower performance. In contrast, the CO2 conversion rates of MoS2–N2H4-4 and MoS2–N2H4-8 were almost equal. In conclusion, the addition amount of hydrazine hydrate can affect the conversion rate of CO2, but its effect gradually decreases after reaching a certain amount. Therefore, MoS2–N2H4-4 is considered to be the most appropriate catalyst for the addition of hydrazine hydrate.
The influence of GHSV was also investigated using the MoS2–N2H4-4 catalyst at 220 °C (Fig. 5a). As the GHSV increased, the conversion of CO2 decreased, while the selectivity of methanol and STYCH3OH increased. This indicates that at high GHSV, the residence time of the reactants is short and the RWGS reaction is limited. When the reaction pressure increases from 3 MPa to 5 MPa, both CO2 conversion and methanol selectivity are improved (Fig. S11†). Considering the CO2 conversion rate and the mild experimental conditions, we determined the optimized GHSV of 8000 mL gcat−1 h−1 and pressure of 4 MPa, as the basis for this study. According to the Arrhenius formula, the apparent activation energy (Ea) of the three catalysts (MoS2–N2H4, MoS2–NH3, and MoS2–NaPH4) was calculated (Fig. S12†), and the results showed that MoS2–N2H4 had the lowest Ea, indicating that it had the greatest advantage in reaction kinetics. However, MoS2–NaPH4 has the lowest Ea and the slowest reaction rate, which conforms to the performance law.
The long-term stability of the MoS2–N2H4-4 catalyst was tested for a total of 200 h at 220 °C (Fig. 5b). In the initial phase of CO2 conversion using the MoS2–N2H4-4 catalyst, the CO2 conversion and methanol selectivity showed a slow upward trend and stabilized at about 5.8% and 77%, respectively, after 20 hours. This suggests that the reducing environment of the reaction contributes to Sv formation. As the reaction time was extended to 200 h, the CO2 conversion rate, methanol selectivity and STYCH3OH showed no sign of weakening, indicating that MoS2–N2H4-4 possesses excellent stability. According to the SEM results (Fig. S13†), the nanoflower structure of MoS2–N2H4-4 remained good after long-term testing. The XRD pattern of the catalyst after the reaction (Fig. S14†) shows that the diffraction peak is almost the same as that of the fresh catalyst before the test, which proves that the MoS2–N2H4-4 catalyst has excellent structural stability. Comparing the XPS spectra of the catalyst MoS2–N2H4-4 before and after the reaction (Fig. S15†), it was found that the proportion of the Moδ+ peak area increased slightly, confirming that the reducing environment has increased Sv, consistent with the long-term stability performance test (Fig. 5b). The comparison of MoS2–N2H4-4 catalysts with reported methanol synthesis (Table S2†) showed that the prepared catalysts in this study have good CO2 hydrogenation performance.
The CO2-TPD technique was used to compare the CO2 adsorption capacity of all catalysts to explain the increased catalytic activities. To elucidate the reasons for the change of the CO2 conversion rate, the CO2 desorption peak in the 200–500 °C region was analysed, and the results are shown in Fig. 5c and S16.† It was found that the peak area of the catalyst decreased successively: MoS2–N2H4-4 > MoS2–NH3 > MoS2 > MoS2–NaBH4, which was consistent with the trend of the CO2 conversion rate in Fig. 4b. Therefore, the high CO2 conversion rate of the MoS2–N2H4-4 catalyst was due to the production of a large number of alkaline sites, which may be caused by the Sv of the catalyst, indicating that the reduction of hydrazine hydrate can enhance the adsorption capacity of CO2. The CO2 adsorption peak of the MoS2–NaBH4 catalyst appears last, indicating that the MoS2–NaBH4 catalyst had the weakest CO2 adsorption/activation capacity. It can be seen that the reductant with stronger reducing capacity is not more favorable to the CO2 hydrogenation reaction. In addition, with the increase of hydrazine hydrate addition, the CO2 adsorption area of MoS2–N2H4-2 and MoS2–N2H4-8 also gradually expanded (Fig. S16†).
The structure–performance relationship of MoS2 treated with different chemical agents is summarized in Fig. 5d, where expanded interlayer spacing and enhanced sulfur vacancies lead to the highest methanol STY. It can also be inferred that by increasing Sv concentration and interlayer spacing, the adsorption of CO2 can be promoted, and the conversion rate of CO2 can be improved. MoS2–N2H4 can release NH4+ to expand the interlayer spacing, and the reducing agent is more conducive to enter the interlayer for reduction, resulting in in-plane Sv, thereby increasing the methanol yield. The methanol yield of expanding the interlayer spacing alone or increasing the Sv alone is lower than that of the combination of the two. Therefore, there is a synergistic effect between the interlayer spacing and the Sv.
Fig. 6 (a) DFT calculated charge density difference diagrams of CO2 adsorption, (b) total density of states, and (c) adsorption energy (Eads) of CO2. |
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4ta02861a |
This journal is © The Royal Society of Chemistry 2024 |