Panagiota
Koralli
ab,
Alkmini
D. Nega
a,
Lida Evmorfia
Vagiaki
b,
Aristea
Pavlou
bc,
Michael G.
Siskos
c,
Antonia
Dimitrakopoulou-Strauss
a,
Vasilis G.
Gregoriou
d and
Christos L.
Chochos
*b
aClinical Cooperation Unit Nuclear Medicine, German Cancer Research Center, 69120 Heidelberg, Germany
bInstitute of Chemical Biology, National Hellenic Research Foundation, 48 Vassileos Constantinou Avenue, Athens, 11635, Greece. E-mail: chochos@eie.gr
cDepartment of Chemistry, Section of Organic Chemistry and Biochemistry, University of Ioannina, Ioannina, 45110, Greece
dNational Hellenic Research Foundation, 48 Vassileos Constantinou Avenue, Athens, 11635, Greece
First published on 4th June 2020
The development of new aqueous conjugated polymer nanoparticles with high photoluminescence quantum yields (PLQYs) at the far red and near infrared (NIR) spectral regions (>650 nm) as alternative polymer probes for fluorescence imaging is reported. This is achieved through an appropriate chemical design by the introduction of up to four fluorine atoms in the different positions of a donor–acceptor (D–A) polymer backbone consisting of thiophene as the electron donating unit and quinoxaline as the electron withdrawing building block. The resulting series of low synthetic complexity conjugated polymers enable us to perform a detailed structure–properties relationship study between the synthesized conjugated polymers and their corresponding aqueous nanoparticles as prepared by the nanoprecipitation and encapsulation methods. We manage to achieve PLQY for aqueous NIR conjugated polymer probes of 0.1 and a PLQY of 0.18 for the far-red emitting conjugated polymer probes. Furthermore, our work paves the way for the rational design of new conjugated polymers with enhanced PLQY, especially in the NIR spectral region, through better control of the intramolecular and intermolecular polymer chain interactions.
For these reasons, different types of fluorophores have been developed toward this goal, including small molecule-based fluorophores,8–10 single-walled carbon nanotubes,11,12 semiconductor quantum dots (QD),13,14 and rare earth-doped nanoparticles.15–17 Each material, however, suffers its own limitations, such as the aggregation-caused quenching effect, low quantum yield (QY), poor photobleaching resistance, high cytotoxicity, or long-term retention in the body.18–20 For example, most FDA-approved clinical agents3 (e.g., indocyanine green, 5-aminolevulinic acid, and methylene blue) suffer from irreversible photobleaching and issues of low brightness and small Stokes shifts. As a result, the development of well-designed NIR fluorophores with high brightness, good photostability, and large Stokes shifts is a profound need in modern bioimaging and clinical diagnosis. Conjugated polymer nanoparticles (CPNs) have recently emerged as a new class of fluorescent nanoparticles because their fluorescence properties can be fine-tuned by an appropriate molecular design of conjugated polymers (CPs).21–24 Given their superior fluorescence brightness and photostability as well as low cytotoxicity, the applicability of CPNs as fluorescent tags and sensors has been expanding significantly during the last few years.25–29 Recent studies have demonstrated that, in some cases, the performance of CPNs as fluorescent tags surpasses that of conventional organic dyes and QDs.30,31
A major obstacle in the development of CPNs is that fluorescence quenching sites (i.e., energy trap sites) are generated through aggregate formation by strong interchain or intrachain interactions (e.g., π–π stacking) inside the CP nanoparticles, which results in severe fluorescence quenching (reduction of fluorescence quantum yields).32–35 Fluorescence quenching is more severe in the far-red and NIR emitting conjugated polymers since their extended π-conjugation system often needs fused and polycyclic molecules, leading to increased inter- and intra-chain interactions. To prevent the formation of fluorescence quenching sites and to obtain particles with high fluorescence quantum yields, different approaches have been utilized, such as aggregation-induced emission (AIE),36 the incorporation of a small amount of narrow bandgap monomers into a polyfluorene copolymer37 and the use of conjugated polymers that have bent and twisted conformations.38 While relatively large fluorescence quantum yields have been reported using the AIE approach, incorporating AIE moieties into conjugated polymers is difficult and restricts the flexibility of the molecular design. Similarly, the introduction of the exact composition of a narrow band gap monomer in a polymer backbone from batch to batch is not controllable.
In this contribution, we developed a new family of aqueous CPNs as potential far-red and NIR fluorescence polymer probes with high photoluminescence quantum yields by utilizing simultaneously unfused, less rigid polycyclic monomer building blocks and reducing the planarity of the polymer chains by anchoring fluorine atom(s) as substituents. The synthesized donor–acceptor (D–A) CPs comprise thiophene (T) as the electron donating unit and quinoxaline (Q) as the electron deficient segment in the repeat unit and vary with regards to the number of substituted fluorine atoms (Fig. 1). The formation of CPNs was carried out via both nanoprecipitation and encapsulation methods.39 As an encapsulation polymer, poly(ethylene glycol)methyl ether-poly(lactide-co-glycolide) (mPLGA-b-PEG) diblock copolymer was used. mPLGA-b-PEG is a biodegradable amphiphilic block copolymer approved by both the Food & Drug Administration (FDA) and European Medicine Agency (EMA).40 The size, the morphology and the optical properties of the nanoprecipitated and encapsulated CPNs are thoroughly characterized. This series of CPNs allowed us to perform an extensive structure–property relationship study, by investigating the effect caused by a relatively small change on the chemical structure within the optoelectronic properties of the CPs, as well as on the morphological and optical properties of the produced CPNs. In particular, to the best of our knowledge, a comparison between the two formulation methods for the preparation of CPNs (nanoprecipitation versus encapsulation) has not been performed up to now. The obtained results provide a clear understanding of how the number and the position of the fluorine atoms on the polymer backbone and the formulation method modify the maximum absorption wavelengths, the fluorescence emission characteristics and the photoluminescence quantum yields.
The (3,4-difluorothiophene-2,5-diyl)bis(trimethylstannane) (0.5 mmol) was combined with either the 5,8-dibromo-2,3-bis(3-(octyloxy)phenyl)quinoxaline (0.5 mmol) for the T2fQ or the 5,8-dibromo-6-fluoro-2,3-bis(3-(octyloxy)phenyl)quinoxaline (0.5 mmol) for the T2fQf or the 5,8-dibromo-6,7-difluoro-2,3-bis(3-(octyloxy)phenyl)quinoxaline (0.5 mmol) for the T2fQ2f and the bis(trimethylstannyl)thiophene (0.5 mmol) was combined with either the 5,8-dibromo-2,3-bis(3-(octyloxy)phenyl)quinoxaline (0.5 mmol) for the TQ or the 5,8-dibromo-6-fluoro-2,3-bis(3-(octyloxy)phenyl)quinoxaline (0.5 mmol) for the TQf or the 5,8-dibromo-6,7-difluoro-2,3-bis(3-(octyloxy)phenyl)quinoxaline (0.5 mmol) for the TQ2f. Then, dry toluene (0.025 M) was added to the reaction mixtures. Finally, tris(dibenzylideneacetone)dipalladium(0) [Pd2(dba3)] (0.02 equiv.) and tri(o-tolyl)phosphine [P(o-tol)3] (0.08 equiv.) were added and the reaction mixture was stirred at 120 °C under an argon atmosphere for 24 h. The polymers were purified by precipitation in methanol, filtered and washed using a Soxhlet apparatus with methanol, acetone, hexane and chloroform. The chloroform fractions were evaporated under reduced pressure and the polymers were precipitated in methanol, filtered through a 0.45 mm PTFE filter and finally dried under high vacuum, rendering a dark blue solid for the TQ, TQf and TQ2f and red, orange and yellow solids for the T2fQ, T2fQf and T2fQ2f, respectively. The yields of the resulting polymers are the following: TQ = 88%,TQf = 83%, TQ2f = 76%, T2fQ2 = 91%, T2fQf = 87% and T2fQ2f = 75%.
After their preparation the microemulsions were placed in a suitable glass cell under dust-free conditions. The experimental data were processed using version 6.32 of the Malvern Zetasizer Nano software (Malvern Panalytical Ltd, Enigma Business Park, UK). The temperature during the measurements was constant at 25 °C. Experiments were performed in triplicate for each sample, and the results were presented as average ± S.D.
Φx = Φr(Fx/Fr)·(Ar/Ax)·(nx2/nr2). |
The indexes ‘r’ and ‘x’ are referred to the reference and the unknown sample, respectively.
n (g mol−1) | w (g mol−1) | Đ | λ solmax (nm) | PLsolmax (nm) | PLQY | |
---|---|---|---|---|---|---|
TQ | 19900 | 64200 | 3.2 | 354, 600 | 668 | 0.59 ± 0.04 |
TQf | 11400 | 25800 | 2.3 | 338, 574 | 618 | 0.51 ± 0.02 |
TQ2f | 22600 | 52500 | 2.3 | 319, 557 | 592 | 0.47 ± 0.03 |
T2fQ | 6000 | 11300 | 1.9 | 538 | 600 | 0.37 ± 0.01 |
T2fQf | 8200 | 15600 | 1.9 | 387, 498 | 571 | 0.30 ± 0.01 |
T2fQ2f | 11200 | 16200 | 1.5 | 392, 456 | 544 | 0.22 ± 0.01 |
From the acquired GPC graphs, we can observe that TQ, TQf and TQ2f reveal multiple distinct peaks which correspond to high- and low-molecular-weight components in contrast to T2fQ, T2fQf, and T2fQ2f where only one peak is evident at higher elution times (Fig. 2). This points out that the TQ, TQf and TQ2f polymer chains are adopting mixed extended and aggregated forms in tetrahydrofuran (THF) solution at 25 °C while under the same conditions the T2fQ, T2fQf, and T2fQ2f polymer chains are adopting only the extended form. It seems that the presence of the two fluorine atoms on the thiophene of T2fQ, T2fQf, and T2fQ2f facilitates the solubility of the polymers in THF solution (25 °C) regardless of the number of fluorine atoms present on the quinoxaline moiety.
The absorption and the emission spectra of the TQs in THF solution are presented in Fig. 3, and the corresponding optoelectronic properties are summarized in Table 1. It is revealed that all synthesized polymers exhibit light absorption and fluorescence emission in the UV-Vis region of the spectra. Their optical properties are tunable and are significantly affected by the number and the position of the fluorine atoms anchored on the polymer backbone. The shape of the absorption spectra is qualitatively similar for all polymers, except TQ2f and T2fQ2f which display a different allocation. For each polymer, two major absorption bands are observed in solution, a phenomenon commonly observed for D–A copolymers. The absorption at low-wavelengths can be attributed to the π–π* transition whilst the high-wavelength peak is related to an intramolecular D–A charge transfer.55 All polymers exhibit absorption maxima at low-wavelengths in the range 319–394 nm, whereas the high-wavelength transition is detected in the range between 557 nm and 600 nm for TQ, TQf and TQ2f and between 456 nm and 538 nm for T2fQ, T2fQf, T2fQ2f (Table 1).
A general trend is detected for the high wavelength absorption maxima of the polymers. We noticed a blue shift of the absorption maxima for the high-energy transitions of all polymers upon the incorporation of fluorine atoms on the polymer chain, as compared to the corresponding absorption peak of the non-fluorinated TQ polymer (Fig. 3a). On the other hand, the low-wavelength absorption peak of the polymers presents a different trend. While TQ, TQf and TQ2f show a blue shift of the low wavelength absorption peak upon addition of fluorine atoms on the quinoxaline, T2fQf and T2fQ2f demonstrate a slight (∼5 nm) red shift (Table 1). This indicates that the gradual increase of the fluorine atoms weakens the intramolecular interaction of the D–A charge transfer and for the case of TQ, TQf and TQ2f the stepwise addition of the fluorine atoms in the quinoxaline is altering the locally excited (LE) state, whereas in T2fQ, T2fQf and T2fQ2f the increase of the fluorine atoms on the quinoxaline does not affect the LE state significantly. Interestingly, comparing the two related polymers TQ2f and T2fQ which differ as regards the positioning of the two fluorine atoms (thiophene and quinoxaline) it shows that the absorption maximum of TQ2f is red shifted versus T2fQ. It seems that when the thiophene is substituted with the two fluorine atoms the electron donating property is reduced due to the high electronegativity of the fluorine atoms.56 In addition, the electron withdrawing property of the fluoro-substituted quinoxaline is decreased upon removing the two fluorine atoms. It is therefore expected that the high wavelength absorption peak maxima, assigned to the ICT of the TQ2f, will be red-shifted versus T2fQ. Furthermore, it is obvious that the anchoring of the fluorine atoms on the polymer backbone blue shifts the emission maxima (Table 1). More specifically, TQ, TQf and TQ2f show emission maxima at 668 nm, 618 nm and 592 nm, respectively while T2fQ, T2fQf and T2fQ2f reveal emission maxima at 600 nm, 571 nm and 544 nm, respectively. Contrary to what has been observed for the variation of the absorption maxima between TQ2f and T2fQ, the emission maximum of the T2fQ in solution is red shifted versus TQ2f. Finally, we have calculated the PLQY of the CPs in the THF solution and the results are shown on Fig. 4 and depicted in Table 1. A general trend is observed indicating that as the number of fluorine atoms in the repeat unit increases, the PLQY drops. For instance, the PLQY of the TQ is 0.59 (no fluorine atoms in the repeat unit) and gradually drops to 0.22 for the case of T2fQ2f (four fluorine atoms in the repeat unit).
Fig. 4 Comparison of the photoluminescence quantum yields for the TQ-based polymers in THF and their corresponding aqueous CPNs. |
In this work, we choose to prepare the CPNs with both methods since to the best of our knowledge there are only limited studies that systematically compare the optical properties between the CPNs formed with the nanoprecipitation and encapsulation methods.57–59 For the formation of the CPNs via the nanoprecipitation method (Fig. 5), firstly, each conjugated polymer was dissolved in tetrahydrofuran (THF) which is a low boiling point aprotic polar solvent miscible with water at a concentration of 0.1 mg mL−1. At such low concentrations, the polymer chains usually adopt their extended form. Then, a different portion (from 1 mL to 1.5 mL on a case-by-case basis) of each different polymer THF solution (stock solution) was added dropwise to 7 mL of deionized water followed by sonication at room temperature. For the encapsulation method, 1 mg of each TQ conjugated polymer and 9 mg of poly(ethylene glycol)methyl ether-block-poly(lactide-co-glycolide) (mPEG-b-PLGA) were dissolved in 1 mL of THF. The choice of mPEG-b-PLGA was based on the fact that it is an FDA approved and metabolizable copolymer.40,60 The resulting solutions are added to 7 mL of deionized water following the same procedure as described for the nanoprecipitation method (Fig. 5). In both cases, the solutions were left overnight to allow complete evaporation of the THF and the volume of water lost was replaced. After this procedure, stable aqueous CPNs are formed through aggregate formation of the hydrophobic conjugated polymer chains in the case of nanoprecipitation, whilst by applying the encapsulation method, the hydrophobic PLGA segments are liable to entangle with TQ polymer chains and the hydrophilic PEG chains should extend into the aqueous phase. The obtained CPNs were then filtered through a 0.2 μm cellulose acetate filter. The resulting concentrations (before filtration) of the CPNs prepared via the nanoprecipitation method were 2.8 ppm for the TQ polymer and 4.3 ppm for all the others, and 143 ppm for the CPNs prepared via the encapsulation method.
Fig. 5 Schematic representation of the conjugated polymer nanoparticle preparation through nanoprecipitation (top) and encapsulation (bottom). |
It is important to use different characterization techniques to calculate the size and the distribution of the prepared nanoparticles in order to obtain a more complete view of the CPNs and their behavior. To evaluate the sizes of the formatted aqueous TQ-based polymer nanoparticles dynamic light scattering (DLS) measurements were performed at room temperature, 25 °C, a day after their preparation (Fig. 6 and 7) and the results are depicted in Table 2. The DLS measurements indicate that the aqueous TQ nanoparticles exhibit a unimodal size distribution regardless of their preparation method (Fig. 6 and 7). The majority of the nanoprecipitated CPNs had a hydrodynamic diameter between 30 and 50 nm (Table 2). Nanoparticles that were prepared via the encapsulation method were slightly larger, ranging in size from ca. 50 to 60 nm (Table 2). This observation was expected because of the use of the mPEG-b-PLGA block copolymer.
Fig. 6 Size distribution of aqueous TQ nanoparticles prepared via the nanoprecipitation method determined by DLS measurements and their morphology using TEM. |
Fig. 7 Size distribution of aqueous TQ nanoparticles prepared via the encapsulation method determined by DLS measurements and their morphology using TEM. |
CPNs | Nanoprecipitation | ||||
---|---|---|---|---|---|
Z-Ave. (nm) | PDI | PK1 mean (nm) | Z potential (mV) | TEM | |
TQ | 40.98 ± 0.12 | 0.13 ± 0.01 | 47.26 ± 0.56 | −20.3 | 30.85 ± 2.12 |
TQf | 31.67 ± 0.09 | 0.21 ± 0.01 | 37.80 ± 1.07 | −19.6 | 24.04 ± 1.01 |
TQ2f | 40.55 ± 0.12 | 0.18 ± 0.01 | 46.51 ± 0.48 | −17.7 | 33.74 ± 2.61 |
T2fQ | 48.13 ± 0.31 | 0.17 ± 0.02 | 53.87 ± 3.58 | −21.0 | 33.50 ± 1.45 |
T2fQf | 75.03 ± 1.22 | 0.16 ± 0.02 | 84.65 ± 4.94 | −18.2 | 39.77 ± 3.16 |
T2fQ2f | 33.34 ± 0.15 | 0.21 ± 0.01 | 37.97 ± 0.60 | −15.5 | 27.45 ± 3.11 |
Encapsulation | |||||
---|---|---|---|---|---|
Z-Ave. (nm) | PDI | PK1 mean (nm) | Z potential (mV) | TEM | |
TQ | 57.71 ± 0.20 | 0.11 ± 0.01 | 65.64 ± 0.46 | −10.5 | 17.41 ± 1.82 |
TQf | 57.86 ± 0.20 | 0.12 ± 0.01 | 66.78 ± 0.40 | −11.0 | 19.01 ± 2.06 |
TQ2f | 69.40 ± 0.42 | 0.11 ± 0.01 | 75.54 ± 9.46 | −11.2 | 19.28 ± 1.06 |
T2fQ | 52.46 ± 0.15 | 0.12 ± 0.01 | 60.13 ± 0.41 | −10.7 | 17.40 ± 0.74 |
T2fQf | 52.26 ± 0.16 | 0.11 ± 0.01 | 63.93 ± 0.96 | −10.7 | 19.55 ± 0.91 |
T2fQ2f | 58.32 ± 0.13 | 0.13 ± 0.01 | 69.13 ± 7.22 | −10.3 | 18.65 ± 1.90 |
Interestingly, we notice that the TQ2f nanoparticles prepared using the encapsulation method and the T2fQf nanoparticles prepared via the nanoprecipitation method exhibit hydrodynamic diameters around 70 nm and 75 nm, respectively (Table 2). This observation occurred for all the prepared batches that we examined probably due to their higher tendency to form aggregates based on the reported TEM images. According to the distribution of nanoparticle sizes, those prepared via the encapsulation method demonstrate relatively narrow size distributions with low polydispersity indexes (PDIs) of 0.10–0.13 compared to the PDI of those prepared via the nanoprecipitation method which presented higher PDI values (Table 2).
Simultaneously with the DLS measurements, the zeta potential of the CPNs was measured. The colloidal stability of our aqueous CPNs is confirmed by the substantial and negative zeta potential, as shown in Table 2. It is obvious that the nanoparticles prepared via the nanoprecipitation method display zeta potential values ranging from −15.5 to −21 mV, while the corresponding ones prepared via the encapsulation method exhibit a more neutral zeta potential of approximately −11 mV. The origin of a negative zeta potential has been addressed in previous studies61,62 and it is attributed to oxidative defects on the surface of the CPNs or to the presence of the π-polarizations of the polymer rings that enable stronger attractive van der Waals forces and hydrophobic interactions. Therefore, when the conjugated polymer is encapsulated inside the amphiphilic copolymer, those interactions are minimized resulting in lower zeta potential values.
Transmission electron microscopy was further used to investigate the shape and dimensions of the CPNs (inset of Fig. 6 and 7). The measurements revealed distinguishable approximately spherical shape for all nanoparticles. The median diameters range from 24.04 ± 1.01 nm to 39.77 ± 3.16 nm for the nanoprecipitation method and from 17.40 ± 0.74 nm to 19.55 ± 0.91 nm for the encapsulation method, being in agreement with the DLS measurements according to the narrow size distributions exhibited by the encapsulated CPNs. The difference between the sizes of the nanoparticles observed by TEM versus the DLS measurements can be attributed to the fact that the hydrated size of CPNs in water is typically larger than size measurements obtained in the dry state. This discrepancy has been previously reported.63,64 In both cases, the average particle size was determined to be lower than 100 nm, which is an acceptable size for biological applications, since nanoparticles with sizes >100 nm may have issues such as poor mass transfer, tissue penetration and non-specific absorption.61,65 The resulting sizes and shapes of the prepared CPNs are sufficiently small to be internalized by the cells. Moreover, it has been demonstrated that CPNs larger than 200 nm are excreted via the liver and spleen while for sizes smaller than 10 nm the excretion is performed through the kidneys,66 highlighting the potential application of these CPNs as fluorescent contrast agents.
However, apart from the appropriate size and dimension of the nanoparticles, it is essential to show high photoluminescence quantum yields (PLQYs). It is well known that CPs exhibit inherent hydrophobicity and when they are formulated into nanoparticles in aqueous solution, the tight packing of the polymer chains in the particles results in severe fluorescence quenching, which significantly decreases the PLQY and the brightness of the probes. In this work, we attempted to prevent the strong π–π stacking of the CP chains by decreasing the intramolecular planarity of the polymer backbone through increase of the torsion angle that will occur via the gradual incorporation of fluorine atoms on the thiophene and quinoxaline units. Fig. 8 and 9 present the UV-Vis absorption and fluorescence spectra of the CPNs formulated by nanoprecipitation and encapsulation, and the corresponding UV-Vis absorption and fluorescence maxima are summarized in Table 3 along with the measured PLQY.
Fig. 8 UV-Vis absorption spectra and normalized emission spectra of TQ-based CPNs prepared via the nanoprecipitation method. In the inset of Fig. 8b the nanoprecipitated CPNs in water are shown (from left to right; TQ, TQf, TQ2f, T2fQ, T2fQf, T2fQ2f). |
Fig. 9 UV-Vis absorption spectra and normalized emission spectra of TQ-based CPNs prepared via the encapsulation method. In the inset of Fig. 9b the encapsulated CPNs in water are shown (from left to right; TQ, TQf, TQ2f, T2fQ, T2fQf, T2fQ2f). |
CPNs via nanoprecipitation | CPNs via encapsulation | |||||
---|---|---|---|---|---|---|
λ absmax (nm) | Plmax (nm) | PLQY | λ absmax (nm) | Plmax (nm) | PLQY | |
TQ | 359, 614 | 728 | 0.05 ± 0.03 | 604 | 726 | 0.08 ± 0.01 |
TQf | 358, 612 | 732, 806 | 0.05 ± 0.03 | 362, 603 | 734 | 0.09 ± 0.01 |
TQ2f | 357, 587 | 744, 812 | 0.06 ± 0.01 | 353, 582 | 744 | 0.05 ± 0.01 |
T2fQ | 555 | 690 | 0.10 ± 0.02 | 555 | 683 | 0.07 ± 0.01 |
T2fQf | 518 | 692 | 0.18 ± 0.04 | 397, 515 | 662 | 0.17 ± 0.01 |
T2fQ2f | 394, 474 | 647 | 0.18 ± 0.01 | 397, 471 | 650 | 0.16 ± 0.02 |
It is revealed that all CPNs demonstrate a red shift in both absorption and emission maxima in comparison to the CPs in THF. This supports evidence of effective π–π stacking of the polymer chains passing from the extended form in THF to a more aggregate conformation, in the form of spherical species, in the aqueous nanoparticles.61,67 In general, we observe that on the one hand the CPNs substituted by the two fluorine atoms on the thiophene unit (T2fQ, T2fQf and T2fQ2f) exhibit absorption at the UV-Vis and fluorescence emission at the far-red part of the UV-Vis region. On the other hand, the CPNs not substituted with fluorine atoms on the thiophene unit (TQ, TQf, and TQ2f) present absorption maxima at the UV-Vis to far-red wavelengths and fluorescence peak maxima in the far-red and NIR spectral regions with emission tails extending up to 900 nm (Fig. 8 and 9). These observations are irrespective of the preparation method followed for the CPNs.68
In more detail, it is demonstrated that the low- and high-wavelength absorption peaks of all CPNs and the shape of the absorption profiles do not alter significantly independent of the preparation method, only the optical density is affected. The encapsulated CPNs present higher optical density than the nanoprecipitated ones due to the significantly higher concentration of the CPs loaded in the mPLGA-b-PEG (143 ppm) versus the lower concentration of the nanoprecipitated CPNs (2.8 or 4.3 ppm). Moreover, the same trend observed in solution for all CPs regarding the variation of the absorption maxima of both the low- and high-wavelength peaks as a function of the number of fluorine atoms is also present in the CPNs as well.69,70
Studying the photoluminescence properties of the CPNs as compared to the CPs in THF a controversial effect is revealed. The emission maxima of the CPs in THF are blue shifted upon the addition of fluorine atom(s) on the quinoxaline, regardless of the presence or not of fluorine atom(s) on the thiophene. However, the TQ, TQf, and TQ2f nanoparticles present red-shifted emission maxima whereas the T2fQ, T2fQf and T2fQ2f nanoparticles show blue shifted emission maxima with the gradual increase of the fluorine atom(s) on the quinoxaline independent of the preparation method (Tables 1 and 3). For example, the gradual introduction of fluorine atoms on the quinoxaline moiety of the TQ polymer red shifts the emission maxima of the TQ, TQf and TQ2f CPNs from 726 nm to 744 nm, while by anchoring two fluorine atoms on the thiophene and further adding fluorine atoms to the polymer chain blue shifts the emission peaks at lower wavelengths; from 690 nm to 647 nm in the case of nanoprecipitation and from 683 nm to 650 nm for the encapsulation method. This indicates that even though the self-assembly of the CPs in the CPNs leads to efficient π–π stacking, the number and the positioning of the fluorine atoms plays an essential role in the intra- and inter-chain interactions.
In parallel, we proceed to the measurement of the photoluminescence quantum yield values (PLQY) of the CPNs which are presented in Fig. 4 and depicted in Table 3. The PLQY of the TQ, TQf, TQ2f and T2fQ in THF is significantly higher and the PLQY of the T2fQf and T2fQ2f in THF is higher versus the corresponding CPNs in water (both in the encapsulation and the nanoprecipitation method) as shown in Fig. 4. This confirms our statement that the π–π* stacking of the polymer chains during the nanoparticle formation leads in an increased number of fluorescence quenching sites, especially in the case of TQ, TQf, TQ2f and T2fQ and to a lesser extent in T2fQf and T2fQ2f. In particular, the far-red emitting T2fQf and T2fQ2f nanoparticles exhibit the highest PLQYs independent of the preparation method with values of 0.16–0.18, slightly lower than the corresponding CPs in THF solution (0.30 and 0.22) and blue shifted emission maxima upon gradual increase of the fluorine atoms on the quinoxaline independent of the preparation method. These observations suggest that as the fluorine atoms on the quinoxaline increase the intramolecular disorder increases (in accordance with the theoretically predicted calculations on the dihedral angles in Fig. 10) and the intermolecular interactions between the polymer chains decreases. On the contrary, the NIR emitting CPNs exhibit PLQY up to 0.1. This may be attributed to the fact that the fluorescence quantum yield for NIR emitters are inherently lower than those of UV-visible and far-red emitters as a result of a smaller energy gap between the ground state and emitting state, often making non-radiative relaxation pathways competitive with radiative relaxation.61
In general, the PLQYs of the TQ, TQf and TQ2f nanoparticles are similar within the statistical error regardless of the preparation method. Moreover, the PLQYs of the T2fQ, T2fQf and T2fQ2f nanoparticles are higher than those of TQ, TQf and TQ2f nanoparticles in both preparation methods, except from the T2fQ based nanoparticles prepared via the encapsulation method. Between the T2fQ, T2fQf and T2fQ2f nanoparticles, the PLQYs of the T2fQf and T2fQ2f are similar regardless of the preparation method, whereas the PLQY of the nanoprecipitated T2fQ based nanoparticles is higher versus the encapsulated T2fQ based nanoparticles. These observations lead to the point that the TQ, TQf, TQ2f and T2fQ based nanoparticles exhibit comparable interchain interactions, while the T2fQf and T2fQ2f reveal slightly weaker interchain interactions independent of the preparation method. The fact that the absorption and emission spectra of the nanoparticles prepared from both methods are red-shifted versus the corresponding CPs in THF solution supports the above observation.