State Key Laboratory of Crystal Materials, Institute of Crystal Materials, Shandong University, Jinan 250100, P. R. China. E-mail: zgd@sdu.edu.cn; txt@sdu.edu.cn
First published on 13th June 2023
All-inorganic perovskite CsPbBr3 has been regarded as a new semiconductor radiation material with great potential due to its excellent carrier transport performance and thermal stability. However, it remains challenging to optimize the size and quality of CsPbBr3 single crystals for commercial applications. Here, the [100], [010], and [001] orientations of bulk CsPbBr3 single crystals were examined, and their anisotropic X-ray detection performance was investigated. The regular positive and negative charge distributions at the outer (010) surface and the connection of [PbBr6]4− octahedrons with the [010] orientation contribute to decreased defect densities and enhanced carrier transportation of the (010) facet. Additionally, the wafer with the [010] orientation exhibited the weakest ion migration among the three orientations due to the largest active energy (143.77 meV) and ion diffusion barrier energy (0.361 eV), which is advantageous for enhancing the X-ray response. Moreover, the (010) CsPbBr3 single crystal detector, which was fabricated with EGaIn and Au electrons, demonstrated the maximum sensitivity of 34449 μC Gyair−1 cm−2 under a high bias voltage of −400 V and the lowest detection limit of 52.6 nGyair s−1 compared with the other two devices. This work highlights the anisotropic engineering of large-size single crystals for boosting perovskite radiation performance and provides valuable advice for the oriented growth of large-size crystals and films.
Lead halide perovskite materials have been developed over the past few decades, and they currently exhibit outstanding performance in solar cells,7 photodetectors,8 light-emitting diodes (LEDs),9 lasers,10 and nuclear radiation detectors1,2,11,12 because of their large average atomic number, tunable bandgap, and high mobility-lifetime (μτ) products as well as relatively high resistivity.13,14 In particular, all-inorganic lead halide perovskite CsPbBr3 is useful in radiation detection due to its superior photoelectric properties, as well as satisfactory thermal and moisture stability.10 There is a smaller leak current for a single crystal (SC) of CsPbBr3, which results in high purity in materials, a free grain boundary, and more optimal carrier transport properties compared with polycrystalline perovskite thin films and nanocrystals.15,16
Recently, Kanatzidis et al. reported a high-energy resolution of 1.4% for 137Cs 662 keV γ-ray irradiation based on the CsPbBr3 SC, which is comparable with the CZT detector. Hence, the CsPbBr3 SC is regarded as one of the new-generation high-energy nuclear radiation detectors.10 Toufanian et al. reported on the growth of a large-size CsPbBr3 SC for γ-ray detection with a high-energy resolution of 2% at 662 keV for 137Cs,17 which further verifies its excellent nuclear irradiation performance.
In addition to γ-ray detection, a spectrometer-grade melt-grown CsPbBr3 detector was applied for X-ray detection, whose sensitivity varied between a few tens to over 8000 μC Gyair−1 cm−2, and the detectable dose rate was as low as 0.02 nGyair s−1.18 Moreover, the CsPbBr3 SC detector demonstrated high potential in X-ray photo-counting applications for medical diagnostics, with high energy response linearity, high energy resolution, large count rate, and negligible polarization.19 Nonetheless, the commercial applicability of CsPbBr3 remains hampered by the inability to grow large-size SCs and the difficulties with optimization of the detection performance.
The anisotropy of SC perovskite has a relative impact on the transport of charge carriers and the optoelectronic properties according to the orientation of the atoms in the crystal lattice.15,20–22 Therefore, exploring the anisotropic properties of perovskite SCs is one of the most efficient methods to enhance detection performance. Some groups have reported the anisotropy of tetragonal MAPbI3 and cubic MAPbBr3 hybrid perovskite SCs. The (110) plane in the MAPbI3 SC exhibited low defect densities due to the orientations of the MA+ dipoles and the stacking of [PbI6]4− octahedrons, which decreased the dark current and increased the photocurrents.23 Compared with the (100) facet, there was higher ionic conductivity and larger optical current in the (111) facet in the MAPbBr3 SC, in which the MA+ and Br− ion density was higher.24
CsPbBr3 crystallizes as an orthorhombic structure with a Pnma space group at room temperature. Therefore, CsPbBr3 single crystals will exhibit intense anisotropic optoelectronic properties. Dong et al. precisely fabricated (100) and (111) surface anisotropy of CsPbBr3 single crystals and demonstrated that the carrier mobility of the (100) facet was up to 241 μm2 V−1 s−1 higher than that of the polar (111) facet, due to lower surface defect density.7 Our group investigated the optoelectronic anisotropy of bulk CsPbBr3 SC and showed that there was a more optimal photoresponse from the (001) plane with [010] orientation. The radiation detection performance of bulk CsPbBr3 SC in the regions of parallel and vertical growth direction was significantly different.17 However, the relationship between the crystallographic orientations and the high-energy radiation detection performance of CsPbBr3 SCs is rarely explored.
In this work, we report a large CsPbBr3 SC with the size of Φ 36 mm × 50 mm grown using a modified vertical Bridgman (VB) method. The bulk CsPbBr3 single crystals were orientated, and the (100), (010), and (001) wafers were polished for device fabrication. The structural anisotropy of CsPbBr3 demonstrates a low defect density and great charge carrier transport in the (010) facet. Moreover, compared with others, the higher activation energy and ion diffusion barrier indicates a weaker ion migration of the wafer with [010] orientation. Hence, the (010) detector achieved an optimal sensitivity of 34449 μC Gyair−1 cm−2 under a high bias voltage of −400 V and a detection limit of 52.6 nGyair s−1 for 120 keV X-ray detection. This work aims to explore the crystal facet with optimal properties that is conducive to the directional growth of large-size crystals and the optimization of X-ray detection performance.
CsPbBr3 single crystals were grown in a homemade dual-temperature zone vertical Bridgman furnace that was reported in our previous work. The upper zone and lower zone of the furnace were set to approximately 640 °C and 300 °C, respectively, and the temperature gradient near the solid–liquid interface was approximately 12 °C h−1. After placing the quart ampoule with the CsPbBr3 polycrystals in the Bridgman furnace, the ampoule was maintained at approximately 640 °C for 6 h to completely melt the polycrystals. Afterward, the ampoule was slowly moved down to the lower zone, at the rate of 0.2 mm h−1. The furnace was cooled to room temperature at the speed of 10–20 °C h−1 after the crystallization.
The as-grown CsPbBr3 single crystals were oriented and cut into wafers with sizes of 4 mm × 4 mm × 1.5 mm using an STX-202A diamond wire-cutting machine. The surfaces of the wafers were polished using a 7000 mesh SiC sandpaper with acetone for lubricating. After polishing, the wafers were immersed in an HBr solution for approximately 60 s to reduce the degree of surface defects. Then, the surface of the sample was washed with toluene to remove the HBr residue.
Current density–voltage (J–V) curves for the EGaIn/CsPbBr3/Au devices were measured by an electric properties measurement system (Keithley 2450, Keithley Instruments, OH, USA) with the bias voltage from −400 to 400 V at various scan rates. Current–time (I–t) curves were measured by an electric properties measurement system (Keithley 6517B, Keithley Instruments, OH, USA).
A tungsten anode X-ray tube (VAREX RAD-14/Leo, Hamamatsu, Shizuoka, Japan) was used as the source with an X-ray beam limiter for 1 × 1 mm2. The X-ray source was operated with an acceleration voltage of 120 keV. The dose rate was changed by adjusting the X-ray tube current from 10 to 25 mA, and the dose rate was calibrated using an X-ray machine multifunctional quality detector (Piranha 655, Piranha, Sweden). A source meter (Keithley 6517B, Keithley Instruments, OH, USA) was used to apply the bias voltage and record the response current. All measurements were performed at room temperature (25 °C) in air.
In addition to purifying the raw materials, cracking must be prevented to obtain large-size CsPbBr3 single crystals. When the temperature gradually decreases from the melting point to room temperature, the phase of CsPbBr3 will change from cubic to tetragonal at 130 °C, and then to orthorhombic at 88 °C. The large thermal expansion coefficient near 130 °C usually results in a severe crack in CsPbBr3 during the cooling process and reduces the quality of the crystal. When the cooling rate was decreased to 10–20 °C h−1, there was less cracking. Fig. 1b shows as-grown CsPbBr3 single crystals with the size of Φ 36 mm × 50 mm. After the bulk CsPbBr3 SC was oriented, the crystal was processed into the (100), (010), and (001) wafers with a thickness of 1.5 mm. The photographs of the wafers in Fig. 1b demonstrate the satisfactory crystallization uniformity of the crystal. The X-ray diffraction (XRD) patterns confirmed the orientations of the wafers (Fig. 1c).
Fig. 2 (a–c) Arrangement of [PbBr6]4− octahedrons in the CsPbBr3 crystal structure, and (d–f) photocurrent fitting curves of the [100], [010], and [001] wafers of CsPbBr3 crystal. |
The relaxation and reordering of Br− anions and Cs+ cations at the terminal surface can diminish the surface energy, according to the Verwey theory.25 Therefore, the arrangement of anions and cations that are terminated in the outmost layer of the (010) facet reduces the surface energy and inhibits defect recombination at the surface. Moreover, the various stacking arrangements of [PbBr6]4− octahedrons for the (100), (010), and (001) facets lead to differences in charge transport properties along different orientations. As for the [100] and [001] orientations (Fig. 2a), there is an alternate array of the Cs+ ions and [PbBr6]4− octahedrons that forms zigzag chains and reduces the overlap of the Br-p orbital, which suppresses the charge transport. In contrast, continuous connections across [PbBr6]4− octahedrons along the [010] orientation result in strong Br–Pb–Br bonds, which is beneficial for carrier transport.
A large mobility lifetime product (μτ) increases the charge collection efficiency and improves detection performance. Fig. 2d–f compares the mobility lifetime products of the (100), (010), and (001) wafers, whose thicknesses were all 1.5 mm. The mobility lifetime products were obtained by fitting the obtained photocurrent curve with the modified Hecht equation:
(1) |
A schematic of the typical charging–discharging process is shown in Fig. S2 (ESI†). A bias was applied on the device to promote the movement of ions, and these ions accumulated at the interface between the crystal and electrode. When the ions achieved stability, the bias was abruptly removed, and ions immediately began to travel backward as a result of the high concentration gradient, causing a negative current. As a result, the decay in the negative current curve can be used to evaluate the ion migration, and the activation energy can be fitted using the Arrhenius function from the I–t curves at various temperatures:
(2) |
First-principles calculations were applied to investigate the anisotropy of ion migration in CsPbBr3. Compared with Pb2+ and Cs+ ions, the Br− ion had the lowest activation energy in CsPbBr3 due to the formation of Br− ion vacancies.26 The insets in Fig. 3d–f present the migration paths for the Br− ion vacancy mechanism along the [100], [010], and [001] orientations. We chose a certain Br ion and calculated energy profiles along [100] (blue), [010] (red), and [001] (black) ionic migration channels. The diffusion barrier of the [010] orientation was calculated as 0.361 eV, which is higher than that of the [100] (0.328 eV) and [001] (0.337 eV) orientations.
This trend is consistent in our experiments, although the experimental results are less than the calculated values due to additional defects in actual crystals, which cause lower activation energy.27 Therefore, the higher activation energy of the (010) wafer and the larger diffusion barrier energy along the [010] orientation demonstrated that there is weaker ion migration for the (010) wafer as compared to the others, which is meaningful for the optimization of the X-ray detection performance in CsPbBr3 devices.
As shown in Fig. 4b, the current density–voltage (J–V) curves of the (100), (010), and (001) wafers based on the same part of the CsPbBr3 SC demonstrated the rectifying characteristics. The (010) wafer presented a lower current density of 0.29 μA cm−2 as compared to those of the (100) wafer (0.36 μA cm−2) and (001) wafer (0.58 μA cm−2) under a bias at −400 V. Fig. 4c and Fig. S6 (ESI†) exhibit time-dependent X-ray responses under 120 keV X-ray photons, with dose rates ranging from 12.23 to 30.73 μGyair s−1 and bias from −10 to −400 V for the (010), (100), and (001) wafers, respectively. When the bias increased to −500 V, the detector demonstrated a severe baseline that was caused by ion migration, as shown in Fig. S7 (ESI†). The sensitivities were calculated using the equation:
(3) |
As shown in Fig. 4d and Fig. S8 (ESI†), the X-ray photocurrent densities of the devices were linearly fitted to the dose rates under various bias voltages, and the sensitivities were calculated as 27638, 34449, and 28421 μC Gyair−1 cm−2 under the voltage of −400 V for the (100), (010), and (001) detectors, respectively. Fig. 4e compares the whole sensitivities under different voltages for 120 keV X-ray photons. The sensitivities of the (010) wafer were higher than those of the (100) and (001) wafers.
As the bias increased from −10 to −400 V, the sensitivities of the EGaIn/CsPbBr3 SC/Au detectors gradually increased until saturation (Fig. 4f). The high electric field promotes the diffusion of charge carriers and improves the collection of charges. Once the voltage reaches a certain value, the photoinduced charges are completely collected so that there is saturation of the photocurrent.28 The optimum value of 34449 μC Gyair−1 cm−2 for the (010) detector under the highest bias at −400 V (corresponding to the electric field of −2666 V cm−1) is due to the large μτ product and weak ion migration among the (100), (010), and (001) facets of a single crystal of CsPbBr3. In addition, the sensitivity of the (010) facet detector is three orders of magnitude higher than that of commercial semiconductor α-Se (20 μC Gyair−1 cm−2)2, and five times higher than that of the CZT detector (6069 μC Gyair−1 cm−2).29
Compared with perovskite materials, the sensitivity value is one order of magnitude higher than that of the MAPbI3 detector (1471.7 μC Gyair−1 cm−2)30 and CsPbI3 detector (2370 μC Gyair−1 cm−2),31 and two orders of magnitude higher than that of the FAPbI3 detector (130 μC Gyair−1 cm−2)32 and MAPbBr3 detector (6169 μC Gyair−1 cm−2).33
The current drift D was applied to investigate the stability of the detectors, which is calculated as:
D = (Jt − J0)/(t·E) | (4) |
The detection limit, which was defined as the dose rate with a signal-to-noise (SNR) value of 3, is another important parameter to use for evaluating the performance of the X-ray device. The SNR ratio of the device under various dose rates can be calculated, as follows:
(5) |
Fig. 5e compares the detection limits of three wafers, which were derived from the fitting line with an SNR of 3. The (010) device exhibited the lowest detection limit of 52.6 nGyair s−1, which was approximately two orders of magnitude lower than the standard medical diagnostic requirement of 5.5 μGyair s−1.1 Moreover, the detection limit of our CsPbBr3 SC is two times lower than that of the CZT detector (145 nGyair s−1),29 and four times lower than that of the CsPbI3 detector (219 nGyair s−1),31 MAPbBr3 detector (271 nGyair s−1),33 and FAPbBr3 detector (300 nGyair s−1).32
Fig. 5f and Table 1 compare the X-ray detection performance of reported commercial semiconductors and perovskites. It reveals that our (010) facet of the CsPbBr3 SC device displays the highest sensitivity and the lowest detection limit compared to other reported SC devices. Moreover, our CsPbBr3 SC device exhibited long-term stability under ambient conditions for 10 days with negligible change even when the air humidity reached 60% (Fig. S9, ESI†). In summary, the (010) wafer in CsPbBr3 SC demonstrated optimal X-ray detection properties including high sensitivity, low detection limit, large ion activation energy, and small current drift, providing an approach to optimize X-ray detection devices by controlling the orientations of crystals.
Device structure | X-ray source (keV) | Electric field (V cm−1) | Sensitivity (μC Gyair−1 cm−2) | Detection limit (nGyair s−1) | Ref. |
---|---|---|---|---|---|
α-Se | 20 | — | 20 | 5500 | 2 |
Au/CZT SC/Au | 120 | 5000 | 6069 | 145 | 29 |
Au/MAPbI3 SC/Au | 100 | 33 | 1471.7 | 46000 | 30 |
Au/CsPbI3 SC/Au | 50 | 41.7 | 2370 | 219 | 31 |
Au/MAPbBr3 SC/Au | 120 | 150 | 6169 | 271 | 33 |
Au/FAPbBr3 SC/Au | 50 | 50 | 130 | 300 | 32 |
EGaIn/(100) CsPbBr3 SC/Au | 120 | 2666 | 27638 | 62.7 | This work |
EGaIn/(010) CsPbBr3 SC/Au | 120 | 2666 | 34449 | 52.6 | This work |
EGaIn/(001) CsPbBr3 SC/Au | 120 | 2666 | 28421 | 69.4 | This work |
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3tc01085f |
‡ These authors contributed equally to this work. |
This journal is © The Royal Society of Chemistry 2023 |