First published on 19th October 2023
The timespans over which different plastics degrade in the environment are poorly understood. This study aimed to rank the degradation speed of five widespread plastic polymers–low density polyethylene (LDPE), polypropylene (PP), polystyrene (PS), polylactic acid (PLA) and polyethylene terephthalate (PET)–in terms of their physicochemical properties. Five of the six samples were plastic films with identical dimensions, which allowed the influence of morphology to be excluded, with a polyethylene carrier bag (PEB) tested for comparison. An accelerated weathering chamber was used to photochemically degrade samples over 41 days, with degradation monitored via mass loss and changes to carbonyl index, crystallinity and contact angle. The mass loss ranking was PP ≫ LDPE > PEB > PS > PLA > PET. Estimates of the time needed for complete degradation ranged from 0.27 years for PP to 1179 years for PET. Therefore, mass loss in PP proceeded more rapidly than the other polymers, which was unexpected based on previous literature and is plausibly explained by the presence of an unlisted additive which accelerated degradation. Increases in carbonyl index proceeded more rapidly in PP and LDPE than the other polymers tested. However, changes in contact angle and crystallinity did not correspond to the mass loss ranking. Therefore, monitoring the carbonyl index during accelerated weathering trials can indicate which polymers will fragment more quickly. However, alternative approaches are needed to simulate conditions where photooxidation reactions are negligible, such as the ocean floor.
Environmental significanceUnderstanding how quickly different plastics degrade across various environmental compartments is essential to understanding the risks posed by plastic litter. Photodegradation is typically the most important degradation pathway in the presence of sunlight and is often simulated using accelerating weathering trials. This study investigated links between mass loss and physicochemical properties during accelerated weathering of widespread plastic polymers. Mass loss and increases in carbonyl index proceeded more rapidly in polypropylene (PP) and low-density polyethylene (LDPE) than other polymers tested. However, contact angle and crystallinity did not relate to mass loss. Therefore, monitoring the carbonyl index can indicate which plastics will fragment more quickly. However, alternative approaches are needed to simulate conditions where sunlight is negligible, such as the ocean floor. |
The global annual demand for plastics has reached 367 Mt annually,2 while estimates of mismanaged global plastic waste which accumulated in the environment in 2015 ranged from 60–99 Mt.3
The longevity of plastics poses an environmental risk: most of the plastics ever been produced remain in the environment in one form or another.4 Environmental plastics are eventually fragmented into smaller pieces,5–8i.e., microplastics and nanoplastics, which are typically defined as small pieces of plastic debris in the size range from 25 μm to 5 mm and from 1 to 1000 nm respectively.9 Microplastics and nanoplastics can be transported over large distances in freshwater, the marine environment, and atmosphere and have been detected in some of the most remote regions of Earth.8,10 Since they are bioavailable to a larger range of biota, including humans,11 across multiple trophic levels, there is concern about the toxicological risk they pose to environmental and public health.12 Understanding the environmental degradation of plastics is essential to understanding the risks posed by plastic litter, and how this varies depending on the polymer in question. Environmental degradation can release hazardous chemicals added to plastics, such as flame-retardants, stabilizers or plasticizers,13,14 and enhance the sorption of hazardous pollutants such as polycyclic aromatic hydrocarbons (PAHs), e.g., Udenby et al.15
Several weathering processes affect environmental plastics: biodegradation, photodegradation, thermo-oxidative degradation, thermal degradation, hydrolysis16 and mechanical degradation (abrasion). Polymer degradation can be defined as depolymerisation, overall mass loss, or complete mineralization to CO2 and H2O and involves both physical (related to the bulk structure) and chemical (molecular level) changes.6 Environmental plastics will be exposed to one or more degradation mechanisms,17 depending on the relevant environmental compartment. While literature is dominated by plastic litter in the marine environment, a recent study estimated that the amount accumulated in 2015 in soil was actually slightly higher than in the ocean, with urban soils accounting for 33% of modelled total environmental plastic.10 Photodegradation is typically the most important pathway, at least in the presence of sunlight.5,18–21 It acts to weaken and embrittle plastic litter and typically precedes and fragmentation by mechanical forces, e.g., abrasion with sand or rocks, wave action and swelling–deswelling, and eventually biodegradation.5,7,8,22 Conversely, in certain environmental compartments, for example, subtropical saltmarshes where biofilm formation limits transmittance of sunlight, biodegradation and mechanical abrasion can be more prevalent than photodegradation.23
The mechanism and speed of photodegradation depends on the polymer dimensions and other physicochemical properties, as well as the presence of additives.5,6,8 Polyethylene (PE) is relatively resistant to photodegradation due to a lack of chromophores in its polymer backbone (Table 1), though impurities or defects may act as chromophores to initiate photodegradation.7,18 Various types of PE are in widespread use, differentiated by their density;8 combined they represented 30.3% of polymer demand by resin type in the EU27 + 3 in 2020.2 Polypropylene (PP, 19.7% of polymer demand by resin type (Table 1)2) follows a similar degradation pathway to PE, involving free radicals and chain scission.18 Polystyrene (PS, 6.1% of polymer demand for PS and expanded PS combined (Table 1)2) has phenyl rings, which are susceptible to photodegradation (Table 1) but not biodegradation.7,20 Polyethylene terephthalate (PET, 8.4% of polymer demand (Table 1)2) contains ester bonds which are susceptible to cleavage during photodegradation and hydrolysis in the natural environment.18,24 Polylactic acid (PLA) is a bioplastic, i.e. one produced from renewable biomass substrate, rather than petroleum, which is becoming increasingly popular due to its ability to degrade under industrial composting conditions.25 It exhibits similar degradation behaviour to PET.6
Sample code | Material | EU plastic demand2 | Chemical structure |
---|---|---|---|
a For LDPE and LLDPE combined. b For PS and expanded PS combined. | |||
LDPE | Low density polyethylene | 17.4%a | |
PEB | Polyethylene carrier bag | — | As above |
PP | Polypropylene | 19.7% | |
PS | Polystyrene | 6.1%b | |
PET | Polyethylene terephthalate | 8.4% | |
PLA | Polylactic acid | — |
While degradation mechanisms for commonly-used polymers (such as those in Table 1) are well-described, e.g., ref. 7 the timespans over which degradation takes place are poorly understood and unpredictable.6,26 Thus, many unknowns remain around the speed of degradation and persistence of plastic debris in different environmental compartments.5 Min et al.26 used a theoretical approach to predict the degradation of a range of polymers in the marine environment, which highlighted the importance of molecular properties including crystallinity and hydrophobicity. Chamas et al.6 highlighted the dependence of degradation speeds on plastic shape. Since degradation is essentially a surface phenomenon, the rate of mass loss is typically proportional to the surface area of the plastic particle.6 Thus, a HDPE film was predicted to degrade 260 times faster than a fibre of the same mass and crystallinity.6
Because environmental plastic degradation is highly uncertain, potentially occurring over decades, centuries or even millennia, accelerated weathering trials are often used to deliver realistic experimental timeframes, e.g., ref. 24 such methodologies combine exposure to UV radiation, heat and moisture under more extreme conditions than experienced in the environment and were primarily developed to assess material suitability for outdoor applications.27 This work aimed to resolve some of the uncertainties surrounding how long plastics degrade under accelerated weathering conditions. The degradation speeds of six widespread plastics were ranked by monitoring polymer physicochemical properties. An accelerated weathering chamber was used to photochemically degrade samples in this presence of humidity, i.e., under conditions representative of the terrestrial environment. Five of the samples tested were plastic films of identical dimensions, which allowed us to exclude the influence of morphology on degradation speed. This approach was selected to allow us to test the hypothesis that degradation speed, at least under controlled conditions, is linked to polymer physicochemical properties.
(1) |
(2) |
Peak areas were calculated using SpectraGryph 1.2 spectroscopy software.
(3) |
(4) |
(5) |
Chamas and co-workers subsequently derived an expression for the time needed for complete degradation of the initial polymer piece (td) for a single specific surface degradation rate, assuming constant density and surface area.6 Degradation in this context refers to overall mass loss from the initial polymer piece, which does not necessarily change the total amount of plastic present, as mineralisation is not an implied end result.6
(6) |
Eqn (6) was modified in the current work to account for the two-phase degradation observed experimentally during the study, which comprised of an initialisation and an acceleration phase:
(7) |
Photos of weathered samples revealed subtle physical differences caused by degradation. After 32 days of weathering, the PP and PEB samples, which experienced higher mass loss than the other polymers, exhibited an obvious curl, while there was a slight curl in the LDPE film surface (Fig. 1c). Physical changes in PS film related to changing colour and brittleness (Fig. 1c). Discoloration had started by 16 days of weathering and then rapidly increased over time. It is established that PS exhibits yellowing during photodegradation, caused by the formation of conjugated double bonds40,41 and is considered more susceptible to weathering than PP or PE in the presence of UV-irradiation.7 After 22 days of exposure, obvious cracks and imperfections appeared on the PP film surface, and small cracks on the PEB film surface, whereas the surface of the PE film was little changed. These can be ascribed to the enhanced diffusion of water out from the bulk phase of the PP and PEB films, which generated increased surface area, subsequently leading to enhanced oxidative degradation.42,43
Conversely, the higher increases in crystallinity observed for the LDPE, PEB and PP can be attributed to degradation of the amorphous polymer zones.6,31,46 Plastics such as PE and PP are semi-crystalline materials comprised of micro-scale hard crystallites embedded in a soft amorphous matrix.46 Photo-oxidation takes place almost exclusively in the amorphous zone of plastic polymers.5 On the basis of this, it was expected that PP, which had the highest initial crystallinity of all samples tested of 45 ± 2% (Fig. 2a), would be less degradable, whereas the converse was the case, at least in terms of mass loss. In heavily degraded samples, polymer chain scission and crosslinking reactions are more pronounced47,48 eventually leading to increased brittleness and surface cracking (Fig. 1c).46,49 For instance, for PEB, cracks were observable after 21 days' weathering (Fig. 2b) following a pronounced increase in crystallinity, from 37 ± 2% to 42 ± 1%, between days 10 and 15 of exposure. Regarding PS, over the experimental temperature range (from −10 to 180 °C), the glass transition temperature was observed at ∼103 °C, but there was no evidence of melting (Fig. ESI-2†). Therefore, we were not being able to measure crystallinity for PS samples, suggesting a largely amorphous structure. The glass transition temperature of PS decreased by 4.5 °C after day 26 of weathering (Fig. ESI-2†). Such a decrease is consistent with decreased polymer chain length.6,50 From 32 to 41 days of weathering the glass transition temperature increased by 2.5 °C (Fig. ESI-2†), meaning that after 41 days of exposure, the glass transition temperature had overall decreased by 2 °C, indicative of degradation due to chemical and/or thermal oxidation. DSC plots for the remaining polymers are also shown in Fig. ESI-3† LDPE, PEB, PP and PLA all showed strong positive linear correlations (r ≥ 0.81, see Table ESI-3†) between crystallinity and mass loss.
Regarding PET and PLA, since the FTIR spectra of unweathered samples already exhibited strong bands in the carbonyl region (Fig. ESI-1†), new bands could not be easily detected because they potentially would overlap with existing peaks. Both polymers showed a slight decrease, followed by slight increase, in carbonyl index over the accelerated weathered trial, with overall no notable change (Fig. 4). Nonetheless, FTIR spectra of PET and PLA showed some changes in both the carbonyl group (1712 cm−1) and hydroxyl group (3500 cm−1), which indicates photochemical oxidation reactions were occurring, since both these functionalities are known to be generated during the oxidative reactions during polymer degradation, e.g., ref. 7 FTIR spectra for the other polymers during the accelerated weathering trial are shown in Fig. 3c and ESI-1.†
Changes in contact angle and crystallinity did not correspond to the mass loss ranking. Crystallinity in particular is said to be an important property with respect to polymer degradation.5,6,26 However, PP had the highest initial crystallinity, 45%, of the six samples tested (Fig. 2), which would be expected to reduce degradation speed.
While all films used in the study were purchased on the understanding they were additive free, the supplier subsequently indicated that commercially available PP invariably contains unlisted antioxidant/s designed to prevent degradation during processing (personal communication with Goodfellow), since PP without additives is inherently unstable and will degrade in the presence of air.54 This makes it problematic to obtain additive free PP. The identity of additives present in the PP film was unknown to the supplier, however, phenolic compounds are typically used for this purpose.54 None of the other films contained any UV-stabilisers, colourants or other additives that we are aware of. Thus, the most plausible explanation for the observed mass loss ranking is that the PP sample used contained an unlisted antioxidant additive (see Section 2.1), which acted as a chromophore to initiate and stimulate photochemical weathering. A similar example was recently reported, where Irgafos 168, a widespread phosphite polymer additive which also contains tert-butylphenyl groups55 was found to increase PP degradation by a factor of four after an initialisation phase.56 Similarly, the addition of three low molecular-weight additives – benzophenone, anthraquinone and benzoyl peroxide – accelerated the photodegradation of polystyrene.41 The sample of PP tested in the current study likely contained Irgafos 168 or another additive with a similar impact on degradation.
It is interesting to compare the ranking of polymer mass loss obtained in the current study with relevant literature (Table 2). During accelerated weathering in air then mechanical abrasion by sand, particle release was in the order expanded PS pellet > PP pellet > PE pellet,22 whereas in demineralised water, a PS coffee-cup lid or PLA beverage cup released more particles at two of the three size ranges measured than other plastics studied (PP, PE and PET, Table 2 (ref. 57)). Meanwhile, Chamas et al.6 predicted theoretical mass loss based on 25 references and found that either a LDPE bag or PET water bottle were the fastest degrading plastic, depending on the environmental compartment. Overall, it is notable that there is no consensus in literature regarding the ranking of polymer degradation, even between accelerated weathering studies (e.g., Table 2). However, this is perhaps not surprising given that (i) most other studies do not use samples of standardised dimensions (ii) experimental weathering conditions vary and (iii) additives are typically unknown and can have contradictory effects on degradation speed.
The specific surface degradation rate (SSDR or kd) was introduced by Chamas et al.6 as a standardised metric for quantifying the environmental degradation of plastics, which can be used to calculate the time needed for complete degradation (td, see eqn (5)–(7)). In this study SSDR values (Fig. 5) were calculated from experimental mass loss data (eqn (5)). Chamas et al.6 suggested that for thin plastic films, of the type used in this study (0.05 mm thick), surface area and specific surface degradation rate can be regarded as constant during environmental degradation.
Fig. 5 Temporal changes in specific surface degradation rate (SSDR or kd, left) and the time required for total degradation (td, right) for studied polymers. |
Since Fig. 1 demonstrates that the slow initialisation phase lasted until 15 days, this value was taken as the start of the acceleration phase, and td values were calculated using the final time interval of the weathering trial, when mass loss of the acceleration phase was essentially linear (eqn (7), Fig. 1).
Fig. 5 shows that specific surface degradation rates were temporally variable over the timespan of the trial, rather than uniform. Moreover, the assumption of constant surface area is not appropriate once samples enter the acceleration phase, with estimates of td values likely to be overestimates. It should also be remembered that accelerated weathering utilises more extreme conditions than typical of real-life, and the degradation reported here is faster than would be experienced by environmental plastics. Thus, calculated td values (Fig. 5) are associated with a relatively high error and are not intended to replicate environmental degradation. Nonetheless, they are helpful for ranking polymer degradation providing and approximate estimates of the time required for complete degradation, which can be refined in future work, for example, by modifying for situations where assumptions of constant surface area and/or density do not apply. Given its dependence on mass loss data, the ranking of td follows (Fig. 5). Values for td ranged from 0.27 years for PP, the fastest degrading polymer, to 1179 years for PET, the slowest degrading polymer (Fig. 5).
In the current study, experimental conditions were eight hours of UV irradiation, followed by four hours of moisture, similar to terrestrial locations with heavy rainfall, e.g., the tropics. However, it is considered unwise to make a quantitative correlation with a real-world scenario without first performing validation using outdoor weathering under relevant conditions.58 Conversely, for submerged plastic particles, such as in sediment or the ocean floor, or those covered in biofilm, photochemical reactions will be negligible and parameters which monitor them (e.g., carbonyl index) are not expected to relate to mass loss. Thus, simulated degradation trials should look beyond accelerated weathering methodologies in such circumstances. For instance, long-term trials under representative environmental conditions, which account for degradation pathways other than photochemical oxidation, e.g., biodegradation. Overall, this study provides baseline information about the accelerated weathering of polymer films under standardised conditions, i.e., samples of the same dimensions and without additives where practicable. More research is required to properly understand the degradation behaviour of commercial plastics containing a representative range of additives, including determining the identity and concentration of additives present. Moreover, the current work illustrates the perils of trying to predict the mass loss of polymers based on polymer physicochemical properties. In most cases the additives present in a plastic product are unknown, as they are unlisted by the manufacturer (and potentially vary between production sites or even batches) and can either accelerate41 or suppress54 polymer degradation. This is likely to make theoretical predictions of environmental polymer degradation inaccurate. Chamas et al.6 admit that extrapolations or predictions of this type “are fraught with uncertainty”. Greater transparency from polymer manufacturers regarding the type and amount of additives present in their products will help to improve the accuracy of future predictions of environmental plastic degradation. A similar point has been made previously about the need for increased transparency regarding chemical identities in polymer regulations.59 In the absence of specific information about the identity of additives present in plastics, experimental weathering trials, rather than theoretical predictions, are arguably required to accurately monitor degradation speed.
• The overall order of mass loss was PP ≫ LDPE > PEB > PS > PLA > PET. Using experimental data to extrapolate the time needed for total mass loss from the initial polymer piece provided estimates from 0.27 years for PP to 1179 years for PET under accelerated weathering conditions.
• Mass loss and increases in carbonyl index proceeded more rapidly in PP and LDPE than the other polymers tested. However, changes in contact angle and crystallinity did not correspond to mass loss. As such, the carbonyl index is an indicator of which polymers will experience mass loss more rapidly.
• To the best of our knowledge, none of the films contained additives, except for PP, which contained an unlisted antioxidant additive believed to have accelerated mass loss. Therefore, this study illustrates the perils of making theoretical predictions of mass loss based on polymer physicochemical properties.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3em00295k |
This journal is © The Royal Society of Chemistry 2023 |