Open Access Article
Xuanbei
Peng‡
a,
Han-Xuan
Liu‡
b,
Yangyu
Zhang‡
a,
Zheng-Qing
Huang
b,
Linlin
Yang
a,
Yafei
Jiang
c,
Xiuyun
Wang
*a,
Lirong
Zheng
d,
Chunran
Chang
b,
Chak-tong
Au
a,
Lilong
Jiang
*a and
Jun
Li
ce
aNational Engineering Research Center of Chemical Fertilizer Catalyst, Fuzhou University, Fuzhou, Fujian 350002, China. E-mail: xywang2017@fzu.edu.cn; jllfzu@sina.cn; jll@fzu.edu.cn
bShaanxi Key Laboratory of Energy Chemical Process Intensification, School of Chemical Engineering and Technology, Xi'an Jiaotong University, Xi'an 710049, China
cDepartment of Chemistry, Southern University of Science and Technology, Shenzhen, China
dInstitute of High Energy Physics, Chinese Academy of Sciences, Beijing, China
eDepartment of Chemistry, Tsinghua University, Beijing, China
First published on 7th April 2021
The desire for a carbon-free society and the continuously increasing demand for clean energy make it valuable to exploit green ammonia (NH3) synthesis that proceeds via the electrolysis driven Haber–Bosch (eHB) process. The key for successful operation is to develop advanced catalysts that can operate under mild conditions with efficacy. The main bottleneck of NH3 synthesis under mild conditions is the known scaling relation in which the feasibility of N2 dissociative adsorption of a catalyst is inversely related to that of the desorption of surface N-containing intermediate species, which leads to the dilemma that NH3 synthesis could not be catalyzed effectively under mild conditions. The present work offers a new strategy via introducing atomically dispersed Ru onto a single Co atom coordinated with pyrrolic N, which forms RuCo dual single-atom active sites. In this system the d-band centers of Ru and Co were both regulated to decouple the scaling relation. Detailed experimental and theoretical investigations demonstrate that the d-bands of Ru and Co both become narrow, and there is a significant overlapping of t2g and eg orbitals as well as the formation of a nearly uniform Co 3d ligand field, making the electronic structure of the Co atom resemble that of a “free-atom”. The “free-Co-atom” acts as a bridge to facilitate electron transfer from pyrrolic N to surface Ru single atoms, which enables the Ru atom to donate electrons to the antibonding π* orbitals of N2, thus resulting in promoted N2 adsorption and activation. Meanwhile, H2 adsorbs dissociatively on the Co center to form a hydride, which can transfer to the Ru site to cause the hydrogenation of the activated N2 to generate N2Hx (x = 1–4) intermediates. The narrow d-band centers of this RuCo catalyst facilitate desorption of surface *NH3 intermediates even at 50 °C. The cooperativity of the RuCo system decouples the sites for the activation of N2 from those for the desorption of *NH3 and *N2Hx intermediates, giving rise to a favorable pathway for efficient NH3 synthesis under mild conditions.
Nowadays, the subsequent NH3 re-conversion to H2 and the handling as well as shipping infrastructure including regulations for transportation are already in place.6 The above process follows a protocol of “renewable power supply → electrolytic H2 production → NH3 synthesis → NH3 storage → H2 energy”, in which efficient utilization of renewable energy for green production of NH3 could be realized to achieve a “zero-loss” seasonal energy storage cycle that is carbon-free.3,13–15 However, the present bottleneck is that NH3 cannot be synthesized under mild conditions. Currently, huge plants are required, and for a plant with an annual capacity of 200
000 tons, the investment is at the scale of US$ 1000–2000 per ton of ammonia.7 The aim is to match the pressure of the NH3 synthetic system with that of the electrolysis system employed for H2 production (<5 MPa, mostly lying in the range of 1.0–3.2 MPa) so as to avoid expensive pressure ramping.15 Therefore, advanced catalysts that are adoptable to an efficient eHB process are urgently needed, which can activate N2 for NH3 synthesis at lower pressure.
The major obstacle of NH3 synthesis under mild conditions is the scaling relation.15–18 In order to achieve NH3 synthesis under mild conditions, great efforts have been devoted to seek catalytic materials that can either lower N2 activation barriers19–21 or circumvent the scaling relationship.5,6,22–27 Previous advanced surface-science and theoretical investigations disclose that d-block transition metals (TMs), such as Re, Mo, Ru, Co and Rh, obey the scaling relationship because their surface d-bands are broad in bulk metals.18,28–31 The d-band center of such metals results in strong binding of N-containing intermediates, which require high temperature to desorb. Upon regulating the surface d-band centers of TMs, it is possible to simultaneously tune the binding energy of N2 adsorption and that of surface N-containing intermediates. By so doing, the scaling relation for TMs can be decoupled. Indeed, the surface d-band of a metal-based catalyst can be effectively tuned through the strategy of single-atom catalysts (SACs)32–34 or single-cluster catalysts (SCCs),23,35 leading to d-band adsorption modes different from those of pure metals and conventional alloy compositions.36,37 The unusual electronic behavior of SACs and SCCs could also change the adsorption properties and bonding abilities of each metal atom,30,38 resulting in significant deviations from the scaling relationship.36,39,40 Among the SCCs, dual single-atom catalysts (DSACs) offer the simplest active sites for catalytic reactions.
For the well-known active Ru and Co metals in NH3 synthesis, the Co d-band is narrower than that of Ru because of the quantum primogenic effect,41 resulting in the N2 dissociative adsorption energy of Co being much lower than that of Ru. Despite the fact that the state-of-the-art Ru metal catalysts are efficient for NH3 synthesis, the loading and high cost limit the large-scale use of the noble metal. It is hence advantageous to achieve efficient utilization of Ru by having a small amount of Ru atomically dispersed on atomistic Co to generate a RuCo DSAC. It is expected that the surface d-bands of the two metal atoms could be regulated through the formation of a DSAC, resulting in unique electronic and/or geometric features different from those of monometallic Ru and Co metals.42–44 As there is so far no experimental demonstration on the use of DSACs for NH3 synthesis, we are interested in exploring whether the RuCo DSAC is capable of decoupling the scaling relationship and which mechanism this DSAC system might adopt. Especially, the following issues deserve investigation: (1) the existing form of dual active centers, (2) the state of the surface d-band, (3) the pathway of N2 activation and dissociation, and (4) how to decouple the scaling relation.
Herein, we report the preparation of a RuCo DSAC by introducing a Ru atom on a surface layer of Co–N–C material with Co atoms coordinated by a pyrrolic N of g-C3N4. It is found that with Ru atomically anchored on the surface of single-site Co, there is significant overlapping of Co t2g and eg orbitals, resulting in an electronic structure resembling that of a “free” Co atom. Our experimental and theoretical studies demonstrate that the cooperativity of Ru and Co dual single-atom active centers could decouple the scaling relationship by separating N2 adsorption and activation (on the Ru sites) from H2 dissociative adsorption as well as N-containing intermediate species (mainly *N2H4 and *NH3) desorption (on the Co sites). By so doing, the scaling relation over RuCo DSAC in NH3 synthesis can be decoupled, and the developed RuCo DSAC could efficiently promote NH3 synthesis at 200 °C, giving an NH3 synthesis rate of up to 1.24 mmolNH3 gcat−1 h−1. We believe the acquired understanding can help to accomplish rational design of transition-metal-based DSACs for the decoupling of the scaling relation to achieve high catalytic efficiency under mild conditions as well as to develop advanced catalysts to achieve pressure matching between the electrolysis and catalytic systems in eHB technology.
According to the AC-STEM results, there is distribution of Ru single atoms as well as small clusters on Ru/N–C (Fig. 1c and d, and S4a–d†); the latter is a result of Ru aggregation as indicated by the individual bright dots of different intensity levels. Moreover, the AC-STEM images (Fig. 1e and f, and S5a–d†) taken at different regions of Co SAC show the predominant presence of Co single atoms (Fig. 1e and f, and S5a–d, related descriptions are provided in the ESI†). Interestingly, RuCo DSAC exhibits many individual bright dots (Fig. 1g and h). The dots over RuCo DSAC are repeatedly found at different magnifications (Fig. S6a–c†). Most of these dots show no obvious difference (Fig. 1g and h), and the results show that Ru and Co are uniformly dispersed. The result agrees with the fact that there is formation of dual single-atom Ru and Co as confirmed by extended X-ray absorption fine structure (EXAFS) measurements over RuCo DSAC. The conclusion is in accordance with the fact that there is a Ru–Ru bond attributable to Ru clusters as revealed by EXAFS measurements over Ru/N–C (Fig. S7†).
The EXAFS Ru K-edge (Fig. 2a) and Co K-edge (Fig. 2b and S8†) spectra show no obvious Ru–Ru or Co–Co interaction over RuCo DSAC and Co SAC (Fig. S9†), providing direct evidence for the presence of individually isolated Ru and/or Co atoms in the samples. Assignment of signals from 1 to 4 Å in RoCo DSAC is further confirmed by detailed WT-EXAFS wavelet transform plots (Fig. S10†). A WT intensity maximum near 4.5 Å−1 can be assigned to the Co–N contribution. Moreover, the EXAFS fitting curves (Fig. S11a–d†) show that Ru (Fig. S11b†) and Co (Fig. S11d†) atoms over RuCo DSAC are coordinated with nitrogen atoms, and the coordination numbers (CN) of Ru–N and Co–N over RuCo DSAC are 2.9 ± 0.5 and 2.9 ± 0.9 (Table S2†), respectively, while the CN for Co–Ru is around 2.1.
We then performed XPS and XANES measurements to investigate the chemical state of Ru and Co species. XPS study results show that the surface Ru content in the case of RuCo DSAC is close to the total Ru content (total Ru content is determined by ICP-AES measurements). Notably, there is no detection of the Ru 3p signal after deep etching by Ar+ (Table S3†). These results indicate that Ru mainly disperses on the surface of DSAC. Moreover, the energy absorption edge of Ru K-edge XANES over RuCo DSAC (Fig. 2c) is higher than that of Ru foil but lower than that of RuO2, suggesting an oxidation state of Run+ (0 < n < 4) rather than Ru4+ or Ru0.45 Similarly, the Co K-edge XANES spectra (Fig. 2d) show that the absorption edge position of RuCo DSAC locates between that of Co foil and CoO bulk, suggesting that the single Co atom carries positive charge, which is in accord with the XPS Co 2p study (Fig. S12a†). The XPS binding energy (BE) of the Co 2p3/2 peak (Fig. S12a†) over RuCo DSAC is higher than that of Co2+ (779.2 eV), and lower than that of Co3+ (781.0 eV),46 suggesting that the surface Co atom has a hetero-valence state of Co2+ and Co3+. Additionally, the absorption edge of Ru K-edge over RuCo DSAC (Fig. S13†) is lower than that of Ru/N–C, while the BE of the XPS Co 2p3/2 peak for RuCo DSAC is higher than that for Co SAC (Fig. S12a†), indicating that there is electron transfer from Co to Ru via the Ru–Co bond,47 plausibly due to the higher electronegativity of the Ru atom.48 Meanwhile, the XPS Co 2p peaks of the RuCo DSAC sample significantly shift to lower BE values (−1.58 ± 0.7 eV, Fig. S12b†) when it is subject to Ar+ etching at different depths. These observations further suggest electron redistribution via electron transfer from Co to the surface Ru atom.
Owing to the fact that the total electron yield (TEY) is highly surface sensitive, we collected the N K-edge NEXAFS spectra of RuCo DSAC, Co SAC and Ru/N–C to gain insight into the direction of electron transfer (Fig. 3c). Over RuCo DSAC in the range of 397–402 eV, the characteristic π* peaks at 397.5 (peak a), 398.6 (peak b) and 401.2 (peak c) eV can be assigned to pyridinic, pyrrolic and graphitic nitrogen species, respectively.54,55 The presence of the π* peak is attributed to N coordination that involves electron transfer from N to the coordinated metal atom. Based on DFT calculation results including the electron localization function (ELF) (Fig. 3d–f), charge density differences (Fig. 3g and h), and Bader charges (Fig. 3i), it can be confirmed that there is charge transfer from the N atom of g-C3N4 to the Co atom, with loss of negative charge in the former while gain of negative charge in the latter. Then, the Co atom enriched with an electron acts as a bridge to facilitate the transfer of electrons from Co 3d orbitals to the Ru atom.
The extent of electron transfer from Co to Ru is dependent on the nature of the N species involved in the interaction. The chunk in ELF mapping (Fig. 3d–f) demonstrates the electron interaction between Co and Ru, and that the involvement of pyrrolic N species is the strongest (a greener chunk represents weaker electron interaction). The transferred electron density from the nitrogen species to Co and then to Ru follows the order pyrrolic N ≫ graphitic N > pyridinic N species (Table S4†). Taking together the N K-edge NEXAFS results (Fig. 3c), because of the absence of the a peak over Ru/N–C, it is deduced that Ru does not coordinate with pyrrolic N. In a previous study of ours, it was confirmed that single cobalt atoms can anchor and get stabilized on pyrrolic N species.56 Then, Co acts as a bridge to facilitate electron transfer from g-C3N4 through pyrrolic N and Co to the surface Ru atom. Consequently, there is a decrease of N2 adsorption energy, and the N2 molecule adsorbed on Ru shows a negative charge of −0.39 e− (Fig. 3i). As a site for N2 adsorption, the electron-enriched Ru atom readily donates electrons to the antibonding π* orbitals of adsorbed N2, promoting N2 activation via the weakening of the N
N triple bond.
The electron release and/or donation behaviors of RuCo could influence the nature of N2 adsorption and activation, while the binding and desorption energies of N-containing intermediates are closely related with the d-band centers. Therefore, we investigated the d-band center of the RuCo DSAC surface by ultraviolet photoemission spectroscopy (UPS) and projected density of states (PDOS) calculation. The UPS spectrum (Fig. 4a) shows that RuCo DSAC has a d-band width narrower than that of bulk Co and Ru foil.57 Also, the d-band width of RuCo DSAC is obviously narrower than that of traditional RuCo alloy, as revealed in Fig. S15 (for more details see the ESI†). These results strongly suggest that the d bands of Co and Ru in RuCo DSAC are narrow, which is further implied by the results of PDOS calculation (Fig. 4b–e). For RuCo DSAC, the PDOS of Co over RuCo DSAC (Fig. 4c) significantly shifts towards the Fermi level in comparison with that of bulk Co (Fig. 4b), and the corresponding d-band center of Co shifts from −1.30 eV for bulk Co to −1.65 eV for RuCo DSAC (Table S5†). Also, the shift of the d-band center of Co is obviously more than that of Ru. In comparison with bulk Co (Fig. 4g), the PDOS (Fig. 4h) of RuCo DSAC shows that the eg and t2g states of Co in RuCo DSAC are almost degenerate, suggesting almost overlapping t2g and eg PDOS, and there is a nearly uniform coordination field for the Co 3d states. These results imply that the electronic structure of the Co 3d state in RuCo DSAC resembles that of a “free-Co atom”.39 It is expected that such unique electronic structure could promote desorption of N-containing intermediates, and thus have a beneficial influence on low-temperature NH3 synthesis.
000 mL g−1 h−1 as a function of reaction temperature. Obviously, there is only insignificant NH3 production over the C3N4 support within the test temperature range, which is less than 0.04 mmolNH3 gcat−1 h−1 even at 400 °C. Meanwhile, the NH3 synthesis rates over the three samples in the range of 200–400 °C differ significantly (Fig. 5a). The addition of Ru to Co SAC significantly enhances the NH3 synthesis rate (Fig. 5a), and the rate of RuCo DSAC is much higher than that of the monometallic Ru and Co catalysts. For example, the NH3 synthesis rate over RuCo DSAC at 200 °C is 1.24 mmolNH3 gcat−1 h−1, which is 8.2-fold that of monometallic Co SAC (0.15 mmolNH3 gcat−1 h−1). However, there is hardly any activity over Ru/N–C below 350 °C. Also, the RuCo DSAC outperforms the Cs-promoted Ru/C catalyst, which is one of the most active NH3 synthesis catalysts, by 13.6 times at 200 °C (Table S6†). At 400 °C, the NH3 synthesis rate over RuCo DSAC is 11.20 mmolNH3 gcat−1 h−1, which is 2.6-fold and 7.5-fold that of monometallic Co SAC (4.20 mmolNH3 gcat−1 h−1) and monometallic Ru/N–C (1.49 mmolNH3 gcat−1 h−1) catalysts, respectively. It is noteworthy that the outlet CH4 concentration over RuCo DSAC is negligibly low (Fig. S16†) upon the NH3 synthesis at 400 °C for 25 h under 1 MPa, suggesting that under the adopted conditions the RuCo DSAC is highly stable. Moreover, because the Brunauer–Emmett–Teller (BET) surface areas of Ru/N–C (88 m2 g−1) and RuCo DSAC (189 m2 g−1) as determined by N2 adsorption measurements at 77 K (Fig. S17†) are significantly different (Table S1†), we obtained the surface-area-normalized NH3 synthesis rates and made a comparison (Fig. S18†). An NH3 synthesis rate of 6.36 × 10−6 mmol m−2 s−1 was acquired at 350 °C on RuCo DSAC, while that over monometallic Ru/N–C is negligible. To find out whether the N species of the Ru–Co catalyst could be involved in NH3 synthesis, we exposed the Ru–Co catalyst to 75% H2/Ar at 400 °C and 1 MPa, and the cumulative amount of NH3 as a function of time is provided in Fig. S19.† It can be seen that the NH3 synthesis rate first increases to peak at 60 min, and then decreases sharply with time prolonging under a 75% H2/Ar atmosphere. The NH3 synthesis rate is lower than 0.1 mmolNH3 gcat−1 h−1 after 250 min. To further confirm that the NH3 produced mainly originates from the catalytic synthesis of N2 gas rather than the nitrogen source of N-doped carbon support, the NH3 synthesis rate of RuCo DSAC has also been measured at 400 °C and 1 MPa using the feed gas of 75% H2–25% 15N2, instead of 25% N2–75% H2. Our studies show that the NH3 synthesis rate in the presence of 75% H2–25% 15N2 (10.59 mmolNH3 gcat−1 h−1) is slightly lower than that of 75% H2–25% N2 (11.20 mmolNH3 gcat−1 h−1) at 400 °C and 1 MPa (Fig. S20†), showing that the NH3 produced mainly originates from the catalytic synthesis of N2–H2 mixed gases. The H2-TPD-MS experiment was also carried out (Fig. S21†). The signal of m/z = 17 is very close to the baseline, showing that the production of ammonia can be ignored. However, a very weak signal of m/z = 32 can be discerned, indicating that there are only tiny amounts of dynamic N in the catalyst that can be reacted with hydrogen.
In addition, the NH3 synthesis rate over RuCo DSAC at 400 °C exhibits an approximately linear increase from 11.20 to 20.39 mmolNH3 gcat−1 h−1 when the pressure is raised from 1.0 to 5.0 MPa (Fig. S22†). The catalytic performance of RuCo DSAC at such pressure range should permit convenient eHB operation on a large scale. To further reveal the unique intrinsic catalytic activity, we calculated the turnover frequency (TOF). It is well known that Ru and Co entities are both active for NH3 synthesis, and therefore it is difficult to differentiate the catalytic contribution of the two. Herein, TOFM was calculated (more details are provided in the Experimental section) to express catalytic activity on a per-M-active-site basis. Interestingly, TOFRu and TOFCo over RuCo DSAC reach 0.016 s−1 and 6.7 × 10−3 s−1 (Fig. S23†), respectively, at 400 °C, which is 10.7-fold that of monometallic Ru/N–C and 5.8-fold that of Co SAC. Therefore, it is reasonable to attribute the effective formation of NH3 under mild conditions to strong synergism between the dual atomically dispersed Ru and Co active centers.
Previous studies have shown that the addition of a proper promoter to Ru or Co-based catalysts could promote NH3 synthesis.58,59 In the present work, we studied the effect of adding Ba into the best-performing RuCo DSAC (5 wt% against RuCo DSAC) on the NH3 production rate. As displayed in Fig. 5a, the results reveal that the NH3 synthesis rate of Ba/RuCo DSAC is (1.8–3)-fold that of the non-promoted one, depending on the reaction temperature. Surprisingly, when the temperature is 400 °C, the NH3 synthesis rate over Ba/RuCo DSAC is 23.90 mmolNH3 gcat−1 h−1. Moreover, we compared the NH3 synthesis rates of Ba/RuCo DSAC (Table S6†) and RuCo DSAC (Fig. 5b) with those of selected Ru- and Co-based catalysts, and they are superior to those of the conventional Ru- and Co-based catalysts.
The long-term stability test of RuCo DSAC was conducted at 350 °C for 100 h, and its NH3 synthesis rate remains almost constant after a slight decrease at the initial stage (Fig. 5c). The used RuCo DSAC was subject to TEM, HR-TEM, AC-STEM and XRD analyses. The TEM (Fig. S24a and b†) and HR-TEM images (Fig. S24c and d†) of the used RuCo DSAC show no Ru or Co NPs, and the AC-STEM images (Fig. S25a and b†) of the used RuCo DSAC still show a large number of individual bright dots, revealing the retention of the Ru and Co atomic dispersion even after a stability test of 100 h. The XRD patterns (Fig. S26†) of the used Ba/RuCo DSAC and RuCo DSAC samples indicate the absence of Ru or Co phases. One characteristic peak that is related to the g-C3N4 phase can still be observed after the NH3 synthesis reaction, suggesting high thermal stability of g-C3N4. Meanwhile, the H2-TPR (Fig. S27†) profile of the C3N4 support shows no reduction peak below 550 °C. Also, the H2-TPR profile of RuCo DSAC exhibits no reduction peaks below 500 °C. In addition, the Ar-TPD-MS analysis of the as-synthesized fresh catalysts does not show any desorption or decomposition peak below 600 °C (Fig. S28†). These results undoubtedly confirm that the C3N4 support and RuCo DSAC are stable under the reaction for NH3 synthesis. Evidently, the RuCo DSAC is not only active but also stable under the adopted mild conditions for NH3 synthesis.
From these observations and analyses, it follows that *N2H4 is likely the main intermediates under the reaction conditions, and the presence of *N2H4 also suggests that the activation of N2 is more facile via hydrogenation to NNH than via direct dissociation of N
N triple bonds. Moreover, the accumulation of species such as *N2H4 and *NH3 on Ru/N–C and Co SAC will block the sites for further activation of N2 and H2, thus hindering NH3 formation at low temperature over both samples. For RuCo DSAC, the immediate implications of the involvement of the dual single-atom active sites with narrow d-band centers are the interruption of the scaling correlation between the adsorption/activation of N2 and desorption of surface N-containing species, and hence the superior low-temperature NH3 synthesis performance upon the decoupling of scaling correlation.
To illustrate the role of dual single-atom active centers and to deduce the possible reaction pathway over RuCo DSAC, DFT calculations were performed and the calculation results are shown in Fig. 6a–e and S35–S39.† From these results, the Ru atom is the dominant site for N2 adsorption, due to the higher adsorption energy (−0.56 eV, Fig. S36a†) on Ru than on the Co atom (−0.43 eV, Fig. S36c†). Notably, the adsorption of a N2 molecule on a single Ru atom tends to adopt the side-on coordination (Fig. S36a and c†), due to symmetry matching between the π* orbitals of N2 and 3d orbitals of Ru. Then, the adsorbed N2 on the Ru site is more facile to be hydrogenated than direct N2 dissociation. The energy for directly breaking the N
N bond under the active state on the Ru atom is still up to 2.53 eV, indicating difficult direct dissociation. In general, the cleavage of N
N triple bond needs at least two adjacent Ru atoms.69,70 The absence of Ru–Ru ensembles as revealed in EXAFS and AC-STEM analyses over RuCo DSAC implies that the direct dissociation of N2 is unlikely, which is also consistent with the determination of *N2H4 desorption in Ar-TPD measurements (Fig. S31a†). Then, the N2 molecule on the Ru site needs to be activated before the occurrence of hydrogenation (Fig. 6a). The Co site as a bridge accelerates the electron transfer from g-C3N4 to the Ru site, which promotes the donation of 3d electrons from the Ru atom to the π* orbitals of N2 and weakening of N
N bonds as mentioned earlier.69
On the other hand, the dissociative adsorption of H2 over the Co active center of RuCo DSAC is efficient (Fig. S37a–d†), where H2 adsorption is thermodynamically exothermic throughout the entire reaction pathway. Also, the Co atom plays an important role in gathering and activating H2 for N2 hydrogenation at the Ru atom. The above analysis indicates that the adsorption and dissociation of N2 and that of H2 occur at different active sites. The significant advantage of RuCo DSAC is that the competitive adsorption of N2 and H2 can be effectively avoided, as reflected by the positive reaction order of H2 (Fig. 5f). Comparing the charge density differences (Fig. 6c–e) of N2 and H2 co-adsorption on RuCo DSAC (Fig. 6c) and Co or Ru SAC (Fig. 6d and e) sites, electron filling of π* orbitals decreases with the drop of electron density on N2, clearly showing that the existence of H2 poses a negative effect on N2 activation, and it is more obvious in the latter (charge of N2 shift more than 0.7 e−). H2-TPD results (Fig. S30a†) show that the amount of H2 desorption from RuCo DSAC (1.40 mmol g−1) is much higher than the Co coverage, therefore it is reasonable to deduce that there is a spillover of H atoms from the Co atom to Ru active centers.
What follows is the attack of activated N2 on Ru by spillover H atoms to generate N2Hx species. Note that when the N–N bond becomes weak enough the cleavage of the N–N bond and the generation of *NH2 species may take place. Fig. 6a displays the energy profiles of the full pathway for NH3 production (from state i to xxi), and the pathways of N–N bond dissociation (states iii, iv, ix, and xi) and hydrogenation (from state ii to xiii) for comparison. The first hydrogenation step for the generation of *N2H (from state ii to iii) needs to overcome an energy barrier of 1.56 eV, much lower than that of direct N2 breakage (2.53 eV). Upon the formation of *N2H, the N
N bonds are further weakened as indicated by the charge density differences shown in Fig. 6b. Both the hydrogenation of *N2H species and the cleavage of the N–N bond of *N2Hx species are much easier than the direct dissociation of N2, demonstrating the unique function of H atoms for N2 activation (Fig. 6a). Notably, the entire pathway of N2 hydrogenation is in the presence of excessive adsorbed H atoms, and the Ru site with spillover H atoms can keep the adsorption of N2 activated throughout as illustrated in Fig. 6a.
Subsequently, the *N2H species is further hydrogenated to *N2H2, *N2H3 and *N2H4 intermediates with energy barriers in the range of 0.11–1.20 eV. With the stepwise hydrogenation of *N2Hx species, the energy barrier for breaking the N–N bond keeps falling (2.53 eV for *N2, 2.08 eV for *N2H, 2.06 eV for *N2H2, 0.94 eV for *N2H3 and 0.83 eV for *N2H4), showing that N2 hydrogenation is an effective way to sharply weaken the N–N bond. Finally, the indirect cleavage of the *H2N–NH2 bond takes place together with the formation of two *NH2 species. It is noteworthy that the activation energy for *N2H3 dissociation is also lower than that for *N2H3 hydrogenation, thus the cleavage of the N–N bond of *N2H3 is also possible for the generation of the *NH2 intermediate. Then, the transfer of the *NH2 species from the Ru atom to the Co atom is favorable because of the crowding at the Ru site. With active H atoms available on the Co site, further hydrogenation of *NH2 to *NH3 on the Co site is ready to occur. Compared to the Ru site, the Co site is more favorable for NH3 desorption, releasing the first NH3 molecule to the gas phase. It is remarkable that the reaction energies for the generation of the second NH3 on the Co sites and Ru sites are similar (−1.32 eV and −1.34 eV, Fig. 6f), while the desorption energy of *NH3 on the Co atom (0.10 eV) is much lower than that on the Ru atom (0.66 eV), indicating that NH3 desorption from the Co sites is more preferred in comparison to that from the Ru site.
Overall, two significant findings have been acquired in the present study. First, with the Ru and Co dual single-atom active site, a new route for NH3 synthesis is made possible (Fig. 6g), which is essentially different from those of previously reported monometallic Co or Ru catalysts as well as traditional alloy clusters.71,72 According to the results of experimental and theoretical investigations, electron release and/or donation between Ru and Co atoms could promote N2 adsorption and activation as well as hydrogenation, while the narrow d-band centers of Ru and Co allow desorption of surface intermediate species such as *N2H4 and *NH3 at low temperature. Therefore, the superior performance of RuCo DSAC in NH3 synthesis under mild conditions is attributed to the cooperativity of dual single-atom Ru and Co centers. Second, NH3 synthesis over RuCo DSAC proceeds via the associative pathway, similar to that occurring in the cases of metal single atoms,24,57 clusters,23,36 Li-promoted Ru catalysts and Co3Mo3N.73,74 Over the RuCo DSAC in N2 activation to NH3, the step with the highest kinetic barrier is the hydrogenation of N2 to generate *N2H on the Ru site, which is the rate-determining step. After considering the entropy contribution, the entropy contribution in the RDS step is only 0.007 eV. Notably, it was experimentally observed that *N2H4 is the major detected species, which can be ascribed to the fact that the stepwise hydrogenation of *N2H to *N2H2, *N2H3 and *N2H4 has much lower energy barriers than that of the “*N2 + H → *N2H” or “*N2H4 → *2NH2” process. The net outcome is a steady state of *N2H4 presence and hence easy detection of N2H4.
The synthetic procedure of Ru/N–C and Co/N–C SAC was similar to that of RuCo DSAC, except for the absence of CoPc and ruthenium nitrosyl nitrate solution, respectively.
For the Ba-promoted RuCo DSAC, 5 wt% Ba(NO3)2 was added to the RuCo DSAC via an incipient wetness impregnation (IWI) method.
:
8 volumetric ratio) were reduced in a flow of 25% N2–75% H2 at 400 °C for 4 h. Under the conditions for NH3 synthesis in a 25% N2–75% H2 mixture at a WHSV of 60
000 mL g−1 h−1 and a given pressure, the outlet NH3 concentrations were measured using a known amount of diluted H2SO4 solution (1 mol L−1) and analyzed by ion chromatography (Thermo Scientific, DIONEX, ICS-600). Finally, the NH3 synthesis rates were acquired based on the outlet NH3 concentrations. Turnover frequency (TOFM, M = Co or Ru) was acquired by dividing the NH3 synthesis rate by the total number of Co or Ru atoms.
000 mL g−1 h−1 under a pressure of 1 MPa. The outlet CH4 concentration was detected using an online GC-mass spectrometer (GCMS-QP2010 SE).
Aberration-corrected high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) was conducted on a JEOL JEM-ARM 200 F instrument equipped with a CEOS probe corrector, with a guaranteed resolution of 0.08 nm.
Footnotes |
| † Electronic supplementary information (ESI) available: Experimental details of reference samples, Tables S1–S6, and Fig. S1–S38. See DOI: 10.1039/d1sc00304f |