Shubha
Dubey
*a,
Vipin
Kumar
*bc,
Kumud
Dubey
a,
Chinmay
Sahu
a,
Anchit
Modi
d,
U. K.
Gautam
e,
R. K.
Sharma
e,
Fozia Z.
Haque
f,
Gitanjali
Pagare
g and
N. K.
Gaur
a
aDepartment of Physics, Barkatullah University, Bhopal, 462 026, India. E-mail: shubha.dubey4@gmail.com
bDepartment of Physical Electronics, School of Electrical Engineering, Tel Aviv University, Tel Aviv 699 780, Israel. E-mail: vipinkumar@mail.tau.ac.il; vipinkumar0247@gmail.com
cThe Sackler Center for Computational Molecular and Materials Science, Tel Aviv University, Tel Aviv 699 780, Israel
dDepartment of Basic Sciences, IITM, IES University, Bhopal, 462 044, India
eTechnical Physics Division, Bhabha Atomic Research Centre, Mumbai, 400 085, India
fDepartment of Physics, Maulana Azad National Institute of Technology, Bhopal, 462 003, India
gDepartment of Physics, Sarojini Naidu Govt. Girls PG Autonomous College, Bhopal, 462016, India
First published on 27th August 2024
In the present work, the synthesis of BaZrO3 nano-ceramics is explored through flash combustion utilizing glycine as a fuel. The resulting nanoparticles exhibit a cubic Pm
m space group and a spherical morphology with an average size of 45.31 nm. XRD and EDAX verify the integrity of the phase. FTIR and Raman spectroscopy is used to analyze the molecular bonds and their vibrations, while XPS reveals surface compositions and oxidation states. The electro-optical properties of BaZrO3 are explored through UV-Vis spectroscopy and electronic band structure analysis. The Tauc plot displays a pair of band gaps, with values of 3.08 eV and 3.84 eV, corresponding to indirect and direct characteristics. BaZrO3 demonstrates photocatalytic potential with a degradation efficiency of approximately 36.41% for rhodamine B under visible light. Electronic band structure analysis reveals an indirect band gap of 3.05 eV in BaZrO3. The Bader analysis emphasizes the pronounced covalent characteristics present in the Zr–O bond. Photoluminescence spectra exhibit electronic transitions with a peak observed at 420.57 nm (∼2.94 eV), suggesting activity within the violet light spectrum. The CIE chromaticity coordinates imply prospective uses in the manufacture of violet-blue LEDs. These findings underscore the tailored properties of BaZrO3 nano-ceramics, showcasing their versatility for various applications, notably in advanced optoelectronic devices.
Among the several perovskite nanoparticle varieties, attention has shifted to BaZrO3 nanoparticles due to their ability to emit visible light, making them useful in optical displays and devices.7 BaZrO3 nanoparticles have particular appeal in the realm of optoelectronics owing to their robust efficiency and stability across diverse operational conditions. Furthermore, nanomaterials such as BaZrO3 have unique properties that surpass many standard bulk materials in terms of efficiency and resilience.8,9 Additionally, studies suggest that the BaZrO3 nanoparticles can be used in catalysis, since they have catalytic properties across a wide range of chemical reactions. These nanoparticles not only possess optical prowess but also remarkable traits, such as a simple cubic perovskite structure, demonstrating high chemical stability, exceptional mechanical strength, and resilience to extreme temperatures. These features broaden their utility in fabricating heat-resistant composites. Recent research has unveiled the potential of BaZrO3 nanoparticles as proton conductors.10,11 Zhu and fellow researchers conducted a study aimed at accelerating proton conduction in yttrium (Y)-doped barium zirconate (BaZrO3) through the manipulation of oxygen vacancies. This approach involves engineering these vacancies, primarily achieved by introducing calcium (Ca) doping, with the goal of enhancing proton diffusion within the material.12 The functionality of semiconductor devices, encompassing photon absorption or emission, solid-state lighting, photovoltaic cells, detectors, displays, sensors, lasers, and photocatalysts, is substantially impacted by the bandgap.13 The BaZrO3 perovskite stands as a promising material across diverse applications, ranging from fuel cells to solar photovoltaics, owing to its notable oxide-ion conductivity.14
The bandgap, a fundamental property of semiconductor materials, profoundly influences the functionality of semiconductor devices by imparting unique electrical characteristics essential for modern electronics. It defines the energy distinction between the valence band, where electrons are bound to specific atoms, and the conduction band, housing free electrons capable of mobility within the material, consequently dictating the material's electrical conductivity and optical properties and requiring precise control and modification. Nevertheless, BaZrO3's broad bandgap limits its photoactivity and ability to absorb photons in the visible light spectrum.15 Consequently, modifying BaZrO3's bandgap has become a key area of research to enhance its effectiveness in photovoltaic and related applications. For example, Patra et al. achieved significant improvements in photocatalytic performance by modifying BaZrO3 with carbon dots, demonstrating superior efficiency with an optimal CD loading.6 Various methods have been employed to synthesize BaZrO3 in different sizes and shapes, such as polyhedra, nanocubes, nanowires, decaoctahedra, and monodispersed particles.16,17 These efforts have enhanced its optical, ferroelectric, and electronic properties. Common synthesis techniques include the solid-state reaction (SSR), one-step auto-combustion, sol–gel, precipitation, hydrothermal, and green synthesis techniques, which are widely used to produce BaZrO3 nanoparticles.7,9 Modifying the bandgap of BaZrO3 often involves doping and alloying with specific elements, introducing impurity energy levels into its band structure. This precise synthesis not only affects the size, shape, and composition but also unlocks potential applications in catalysis and microwave technology.18,19 Efforts to enhance visible light absorption in these wide bandgap materials include adjusting their band positions with alternative elements or modifying anions to create oxygen-related vacancies in the lattice structure. Ullah et al. used DFT calculations to analyze the properties of pristine and Cd-substituted BaZrO3, finding that Cd-substitution significantly enhanced optical performance, making it more efficient for optoelectronic devices. Both pure and Cd-substituted BaZrO3 showed potential for efficient overall water splitting, indicating their suitability for green energy applications and solar cells.20 Kayathiri et al.'s green synthesis narrowed BaZrO3's bandgap to 4.01 eV through plant chemical substitution, improving its properties. They reported an 84.1% maximum degradation efficiency of CR dye after 90 minutes of light irradiation.9
However, diverging from traditional doping approaches, an alternative method has been employed in this case, involving modified synthesis techniques, optimized sintering temperatures, and the creation of oxygen vacancies within the lattice.21 High-temperature synthesis techniques offer a means to fine-tune semiconductor bandgaps by tailoring interfacial energetics, adjusting valence and conduction band edges, and inducing surface oxygen vacancies. Surface oxygen voids function as traps for optically generated charge carriers, lessening the likelihood of electron–hole recombination, while bulk oxygen vacancies serve as centers for the recombination of photogenerated charges, significantly impacting photocatalysis.22 In addition, the material experiences the development of mid-gap energy levels as a consequence of these trap states, enabling precise adjustments to the electronic structure. The bandgap values achieved through various synthesis techniques are summarized in Table 1 for a comprehensive comparison.
| S. No. | Composition | Synthesis technique | Sintering temperature | Band gap (eV) | Particle size (nm) | Morphology | Ref. |
|---|---|---|---|---|---|---|---|
| 1 | BaZr1−xCexO3 (x = 0.00–0.04) | Modified hydrothermal method | 100 °C | 2.37–2.14 | ∼150–200 | Hollow spheres | 6 |
| 2 | BaZrO3 | CHM approach | 50 °C | — | 50–240 | Nano cubes | 23 |
| 3 | BaZrO3 | Co precipitation method | 110 °C | 4.87 | 200 | Spheres | 24 |
| 4 | BaZrO3 | Chemically synthesized | 400 °C | 4.28 | 16 | Non-uniform nanoparticles | 9 |
| 5 | BaZrO3 | Green synthesized | 400 °C | 5.3 | 11 | Non-uniform nanoparticles | 9 |
| 6 | BaZrO3 | Pechini-type process | 1100 °C | 4.8 | — | — | 25 |
Our study introduces a novel approach to synthesizing and characterizing BaZrO3 that significantly advances the current understanding and potential applications of this material. We have developed an innovative synthesis method that allows for precise control over both particle size and morphology, addressing scalability and uniformity challenges prevalent in conventional techniques. Moreover, our thorough investigation into impurity phases, employing advanced techniques such as Raman spectroscopy and XPS, provides a deeper understanding of the synthesis process and its implications for materials properties, a level of analysis rarely explored in the existing literature. Crucially, we have demonstrated the capability to finely tune the bandgap of BaZrO3 through careful adjustment of synthesis parameters, essential for optimizing performance in optoelectronic devices. Departing from traditional doping strategies, our approach involves modified synthesis techniques and optimized sintering temperatures to deliberately introduce oxygen vacancies within the lattice, thereby enhancing semiconductor properties. This comprehensive synthesis and characterization approach not only advances fundamental knowledge but also positions BaZrO3 for innovative applications in fields ranging from electronics to catalysis.
Presently, the aim is to tailor the band gap of barium zirconate using suitable synthesis techniques to explore its potential as a photocatalyst for degrading rhodamine B dye and perform a detailed structural, electronic and optical analysis by means of different spectroscopic techniques. Density functional theory calculations, utilizing the projector augmented wave (PAW) method, are employed to confirm the origin of the optical band gap. Bader charge analysis is also performed in order to achieve a quantitative assessment of the bonding characteristics in the BaZrO3 ceramic.
:
0.1
:
0.22 for a one-step facile flash combustion synthesis. The proportional quantities of these materials were determined based on the following chemical equation:![]() | (1) |
The main steps for the one-step facile flash combustion synthesis are schematically illustrated in Fig. 1. The appropriate amount of oxidizers and fuel was taken in a 100 ml beaker and mixed together to form a homogeneous mixture. A sufficient amount of glycine solution was added to ensure that the total number of reducing and oxidizing valences was equal, resulting in an equivalence ratio (oxidizing valences/reducing valences) of one. This served to maximize the release of heat due to the exothermic reaction.
![]() | ||
| Fig. 1 Schematic diagram of the synthesis of BaZrO3 nanoparticles via glycine-assisted combustion techniques. | ||
The obtained homogeneous mixture was then aged overnight at room temperature to form a xerogel. Subsequently, the xerogel was placed on a hotplate and maintained at a temperature of around 200 °C. During this stage, the xerogel underwent dehydration and self-propagating combustion within a few seconds, accompanied by a flash of light. This combustion reaction released CO2 and N2 gases and formed a porous foamy-fluffy powder due to the exothermic reaction between the oxidizer and fuel. The resulting porous foamy-fluffy powder of BaZrO3 was reheated at 250 °C for 4 hours. Afterward, the fluffy powder was ground for 2 hours and calcined at 1200 °C in air for 12 hours using a tubular furnace. Finally, the BaZrO3 powder was reground and sintered at 1200 °C under the same conditions and for the same duration to enhance its crystallinity.
To address surface charging effects, all peaks were referenced to the C 1s spectrum (284.77 eV) in the analysis. The XPS core level spectral data underwent analysis and quantification using XPSPEAK 4.1 software, and the Shirley background method was applied to subtract the background from all XPS spectra. All measurements were conducted at room temperature.
Polarization measurements were performed using ferroelectric hysteresis loops (M/s Radiant Technology, USA) at 20 kHz. The optical band study of synthesized BaZrO3 nanoparticles was carried out using a PerkinElmer Lambda 950 UV-visible spectrophotometer across a wavelength range of 200 to 800 nm. Photocatalytic activity testing of the BaZrO3 catalyst for RhB (10 mg L−1) degradation was conducted under UV light using a 150 W Xenon lamp housed within a column-shaped stainless-steel cabinet (λmax ∼400 nm). Room temperature photoluminescence excitation spectra were acquired using an F-7000 Hitachi fluorescence spectrophotometer, utilizing a Xenon lamp employed as the excitation source for emission.
m (no. 221) space group is presented. The fitting resulted in a final difference and a profile fit. The XRD profile reveals three prominent peaks at 30°, 43°, and 53° with Miller indices (1 1 0), (2 0 0), and (2 1 1), respectively. These observations suggest that the crystal structure is predominantly oriented in the (1 1 0), (2 0 0), and (2 1 1) directions. The calculated pattern and the observed one exhibit a strong correspondence with characteristics atomic parameters after Rietveld refinement are presented in Table 2. The low values of various R-factors such as Rexp, Rbragg, Rp, RF, Rwp, and χ2, along with GOF, support the justification for the refined model, indicating a well-aligned agreement between the experimental data and the refined model.
| Phase | BaZrO 3 | ||||
| Structural & lattice parameters | |||||
| Space group | Pm3m (221) | ||||
| a (Å) | 4.18990 | ||||
| Atoms | Atom | Site/Sym. | x | y | Z |
| Ba | 1b/m m |
0.5 | 0.5 | 0.5 | |
| Zr | 1a/m m |
0.0 | 0.0 | 0.0 | |
| O | 3d/4/mm·m | 0.5 | 0.0 | 0.0 | |
| V (Å 3 ) | 73.5500 | ||||
| D (nm) | 70.2900 | ||||
| ε (×10 −3 ) | 1.6200 | ||||
| 〈d Ba–O 〉 (Å) | 2.96270 | ||||
| 〈d Zr–O 〉 (Å) | 2.09494 | ||||
| Reliability factors | R p | 14.70 | |||
| R wp | 14.70 | ||||
| R exp | 13.94 | ||||
| R Bragg | 1.805 | ||||
| R f | 1.930 | ||||
| χ 2 | 1.120 | ||||
| GOF | 1.054 | ||||
| Elemental composition for BaZrO 3 | |||||
| Element | Weight % | Atomic % | Error % | ||
| C K | 17.1 | 45.3 | 11.4 | ||
| O K | 18.7 | 37.2 | 9.6 | ||
| Zr L | 22.2 | 7.8 | 5.5 | ||
| Ba L | 42.0 | 9.7 | 7.8 | ||
| Total | 100.00 | 100.00 | 34.3 | ||
| Effective Bader charges | |||||
| Atom | Effective Bader charge (e) | ||||
| Ba 2+ | 1.5229 | ||||
| Zr 4+ | 2.4952 | ||||
| O 2− | −1.3394 | ||||
The Williamson–Hall plot method31 was employed to determine the crystallite sizes of the synthesized samples through the following relationship:
β cos θ = 4ε sin θ + kλ/D | (2) |
In Fig. S1(a),† we depict the crystallographic representation of BaZrO3 nanoparticles, emphasizing their perovskite nature characterized by a robust cubic symmetry. In this crystalline arrangement, the central positions are occupied by Ba atoms, with Zr atoms positioned at the unit cell's vertices. Furthermore, oxygen atoms are situated at the midpoint of the edges. Notably, the Ba cations exhibit a 12-fold octahedral coordination, while the Zr cations display a 6-fold octahedral coordination, as illustrated in Fig. S1(b) and S1(c),† respectively, (ESI†).
The analysis of BaZrO3 charge density plots offers crucial insights into its electronic structure and bonding traits. An in-depth examination of the electron density distribution within the unit cell involved conducting a detailed study that mapped electron density in the 110 plane using the GFourier program,32 which is a component of the FullProf package. This method generated two-dimensional Fourier maps, effectively illustrating how electron density envelops each atom in the compound's elements.
Typically depicted with contour lines, these maps offer a clear and intuitive view of electron density distribution. Shown in Fig. S1(d and e),† the color scale in these maps illustrates varying electron density levels. Areas of higher electron density appear in shades of red, while lower density regions are depicted in violet. Significantly, there is a notable elevation in electron density for all atoms except oxygen and the interstitial region. This visual representation effectively illustrates unique electron density patterns for various atoms in the compound, unveiling localized electron distribution and highlighting significant density regions within the crystal structure. From the Pauling electronegativity scale,33 the Ba–O and Zr–O bonds exhibit a more ionic character. Moreover, predominant charge transfer occurs from other atomic species towards the oxygen atoms. Additionally, the Ba–O bond appears more ionic compared to the Zr–O bond.
![]() | ||
| Fig. 4 (a and b) Surface morphology micrographs, (c) average particle size distribution of BaZrO3, and (d) EDAX spectra. | ||
Fig. 4(c) presents the distribution of average particle sizes, with a frequency plot illustrating the size distribution derived from measurements of a substantial quantity of BaZrO3 particles. The particle size distribution conforms to the characteristics of a normal distribution function. Notably, the calculated average particle size of BaZrO3 stands at approximately 45.31 nm. Previously, BaZrO3 powder was synthesized using sol–gel auto-combustion in a pre-heated furnace, exploring the influence of pH variation on citrate nitrate sol-gels and resulting in nanoparticles averaging 33.3 nm in size.36 In order to establish the elemental composition of BaZrO3, Energy Dispersive X-ray Analysis (EDAX) was performed under precisely controlled temperature conditions. The EDAX spectrum depicted in Fig. 4(d) distinctly exhibits the detection of Ba, Zr, and O elements, thus confirming the absence of any significant loss of essential elements during the sintering process, accounting for experimental uncertainties. The elemental composition typical of BaZrO3, involving atomic percentage, is presented in Table 2. This meticulous analytical evaluation reinforces both the consistency in cationic composition within BaZrO3 and the non-existence of secondary phases within the structure of BaZrO3. The observation reveals a Ba/Zr ratio of 1.24, nearly approaching unity, signifying the integration of these elements into the structure and providing confirmation of the absence of any remaining oxides.37
Furthermore, for a thorough comprehension of the elemental composition and distribution within the synthesized nanoparticles, we have incorporated the elemental distribution graphs derived from EDS analysis as depicted in Fig. S2.† The EDS mapping data, shown in Fig. 5(a–d), highlights the following: Fig. 5(a) identifies the region where the EDS mapping was conducted, while Fig. 5(b–d) respectively displays the presence of Ba, Zr, and O in the synthesized sample. Importantly, no other detectable impurities were found within the resolution limit of the EDS measurement.
m phase. Fig. S3† illustrates phonon dispersion relations along the principal symmetry directions of the Brillouin zone. A noteworthy aspect of the phonon spectra is the lowest-frequency phonon branch, which demonstrates negative phonon frequencies at the M-points within the Brillouin zone. The unstable phonon mode at the M-point, which was not observed by Perrichon and coworkers38 or Bilic et al.,39 was detected in other calculations reported by Helal et al.40 and Akbarzadeh,41 which also employed the DFT method. The occurrence of phonon instability at the M-point is contingent upon the selection of the exchange–correlation potential and pseudopotential quality used to depict the interaction between the core and the valence electrons.42
Imaginary frequencies, denoted by negative phonon frequencies, signify a breakdown in crystal symmetry. Anharmonic phonon interactions can also contribute to these negative frequencies, potentially triggering a structural phase transition in BaZrO3 under specific conditions. It is crucial to emphasize that the computed phonon dispersion spectra correspond to conditions of absolute zero temperature and zero pressure. Variations in temperature or pressure can significantly alter the situation. Thus, it can be inferred that BaZrO3 displays dynamic instability at low temperatures and zero pressure. However, this scenario may change under pressure, as evidenced by the previously documented pressure-induced phase transition in BaZrO3 crystals.42–44
Regarding lattice dynamics, this phase transformation corresponds to lattice instability at the Brillouin zone boundary points. The lattice instability identified in the present calculations aligns closely with earlier studies that employed a similar approach.
Raman spectroscopy stands as a remarkably sensitive and robust technique to investigate crystal structures through the analysis of their vibrational bands. By employing group theory analysis, one can ascertain the count of allowed vibrational modes in a specific crystal system. The factor group analysis for pertinent space groups is presented in Table 3.
| Atoms | Site | Symmetry | X | Y | Z | Site species | Irreducible representation |
|---|---|---|---|---|---|---|---|
Pm m space group (Oh1) |
|||||||
| Ba2+ | 1b | O h | 0.5 | 0.5 | 0.5 | F 1u | F 1u |
| Zr4+ | 1a | O h | 0.0 | 0.0 | 0.0 | F 1u | F 1u |
| O2− | 3d | D 4h | 0.5 | 0.0 | 0.0 | A 2u | F 1u |
| E u | F 1u + F2u | ||||||
| Γ Total = 4F1u + F2u | Γ Acaustic = F2u | ||||||
| No Raman active modes | Γ IR = 4F1u | ||||||
Group theoretical studies suggest that perovskite materials with a pure cubic crystal structure do not exhibit first-order Raman active phonon modes in vibrational spectra at room temperature, resulting in the absence of a Raman spectrum.55 However, experimental studies on BaZrO3 samples contradict this, revealing the presence of some Raman active modes or bands (Fig. 6(b)). The literature provides two explanations for the Raman spectrum of simple cubic perovskites. The primary explanation involves second-order scattering, where two phonons with opposite parallel wave vectors undergo allowed transitions, resulting in a low-intensity peak. The less supported explanation attributes the spectrum to the breaking of local symmetry caused by tilt and structural disorder, allowing deviation from the selection rule, and producing active modes in Raman.56 The local symmetry of barium zirconate is influenced by octahedral tilt, oxygen octahedral distortion, or structural instability. Therefore, the observed peaks in BaZrO3 are likely a result of second-order scattering.57,58
Raman active modes are further categorized into two optical components: longitudinal (LO) and transverse (TO). However, in the case of BaZrO3, a perovskite that maintains its cubic phase across all temperatures, it also lacks first-order Raman active modes due to its symmetry constraints. Nevertheless, it exhibits a remarkably intense Raman spectrum, characterized by distinct and well-defined features. This intriguing spectral behavior is likely due to its second-order nature.59Fig. 6(b) depicts the room temperature Raman spectra of the BaZrO3 ceramic. The spectra exhibit a comparable signature, bearing resemblance in their main features to the few spectra reported in the literature.55,56,60–62 The three polar modes in cubic perovskites are commonly referred to as the “Slater” mode, involving an anti-phase motion of the B cation concerning the oxygen octahedra, the “Axe” mode, which entails an anti-phase motion of the apical oxygens with respect to the other oxygen atoms within the octahedra, and the “Last” mode, characterized by an anti-phase motion of the A cation and the ZrO6 octahedra.63 These labels hold particular significance in the context of ferroelectric transitions.63
The Raman spectra of BaZrO3 exhibit distinct bands at approximately 138.75, 357.91, and 691.02 cm−1, which can be attributed to different zone center modes. Specifically, the 138.75 cm−1 band corresponds to the last mode, representing the displacement of Ba relative to the ZrO6 octahedra.64 The 357.91 cm−1 band corresponds to the Slater mode, signifying out-of-plane displacements of Zr in relation to in-plane oxygen atoms. Finally, the 691.02 cm−1 band corresponds to the Axe mode, indicating the displacement of apical oxygens with respect to in-plane oxygens. Additionally, the Raman mode observed at 94.24 cm−1 is associated with the anti-parallel motion of Ba–O. Two first order transverse optical Raman modes, TO2 and TO4 are observed at 170.03 and 549.61 cm−1. Second-order modes are identified at frequencies of approximately 224.58, 412.04 and 589.90 cm−1. Furthermore, three bands are observed at approximately 115.61, 224.58, and 510.29 cm−1, all representing f1u modes. The band at 153 cm−1 aligns with the presence of BaCO3, which may also leave a distinctive mark in XRD analysis. However, we would like to emphasize that the presence of BaCO3 is expected in our synthesis process, and its contribution to the spectra is consistent with its known presence as a precursor. This observation aligns well with previously reported data.55 The mode at 115.61 cm−1 is associated with cation-ZrO3 lattice vibrations, while the mode at 224.58 cm−1 corresponds to O–Zr–O bending vibrations and the mode at 510.29 cm−1 represents Zr–O stretching vibrations. Notably, the last two modes (224.58 and 510.29 cm−1) are independent of the Ba cation. Additionally, the vibrational modes observed at approximately 696.17 cm−1 are associated with distortions occurring at the octahedral site of zirconium within the BaZrO3 unit cell.55–64
![]() | ||
| Fig. 7 (a) XPS survey spectra of BaZrO3 nanoparticles (b) XPS spectra of Ba-3d element, (c) XPS spectra of Zr-3d element, and (d) XPS spectra of O-1s element. | ||
| Atom | Orbital | Binding energy | FWHM | Area | Peak specification |
|---|---|---|---|---|---|
| Ba2+ | 3d | 778.902 | 4.207 | 47 138.09 |
3d5/2 |
| 782.628 | 4.074 | 7550.826 | Surface | ||
| 794.083 | 3.912 | 23 517.36 |
3d3/2 | ||
| 795.418 | 6.845 | 21 014.05 |
Surface | ||
| 805.093 | 6.866 | 7622.065 | Ba-Loss | ||
| Zr4+ | 3p | 175.11 | 3.14 | 1703.944 | Surface |
| 177.54 | 3.06 | 4602.614 | 3d5/2 | ||
| 181.36 | 4.85 | 7983.784 | 3d3/2 | ||
| 184.98 | 2.15 | 773.7342 | Surface | ||
| O2− | 1s | 529.374 | 4.174 | 19 391.94 |
Lattice oxygen |
| 531.850 | 5.306 | 16 481.81 |
O2− vacancy | ||
| 532.330 | 0.792 | 306.157 | Chemisorbed oxygen |
In Fig. 7(c), the HR-XPS spectrum for the Zr 3d orbital is presented. The Zr 3d peaks can be primarily deconvoluted into two components: those around 177.542 eV correspond to Zr 3d5/2, and those at approximately 181.361 eV are attributed to Zr 3d3/2, indicating Zr4+ oxidation states, consistent with the existing literature.68 The observed spin–orbit splitting, i.e., the difference between the binding energy of Zr 3d3/2 and Zr 3d5/2, doublets, (i.e. ΔEBE = BE3d3/2 − BE3d5/2) measures 3.819 eV, aligning with previous findings.70 The presence of spin–orbit split components in the core-level spectra of Ba 3d and Zr 3d, with separations of 15.193 and 3.819 eV, respectively, confirms the +2 and +4 oxidation states of Ba and Zr in the BaZrO3 ceramic.71,72 Peaks observed at 175.110 and 184.984 eV are attributed to oxidized surface species of zirconium.67
Fig. 7(d) presents the high-resolution XPS spectra of oxygen 1s. For pristine BaZrO3, the spectra can be deconvoluted into three peaks at 529.374, 531.850, and 532.330 eV, respectively.73 The characteristic peak of lattice oxygen is evident in the O 1s core-level spectra at 529.374 eV,63 while the peak at 531.850 eV is possibly associated with oxygen vacancies,74 and the peak at 532.330 eV arises due to surface hydroxyl groups.75
The squareness of the ferroelectric ceramic can be determined utilizing the Haertling and Zimmer correlation.
![]() | (3) |
In this context, Rsq represents the squareness parameter of the hysteresis loop. Pr denotes the remanent polarization, Ps indicates the saturated polarization at a finite field strength below dielectric breakdown, and P1.1Ec stands for the polarization at a field equal to 1.1Ec. According to the literature, the ideal square loop (Rsq) of a ceramic equals 2.00. For BaZrO3, the estimated Rsq value is approximately 1.80.
In recent research, the optical properties of BaZrO3 have garnered considerable attention due to its optical band gap, which has been determined to be approximately 4.8 eV using UV-visible spectroscopy.70,71,73 The optical band gap serves as a critical parameter denoting the energy threshold required for photons to be absorbed by the material. It is noteworthy that this optical band gap tends to be somewhat narrower than the corresponding electrical band gap, a characteristic observed in various perovskite oxide materials. This unique feature has stimulated the exploration of BaZrO3's potential in a range of optical applications, particularly in the visible and ultraviolet (UV) spectral regions. The material's substantial band gap, which falls within the range of 3.8 to 7.0 eV, underscores its versatility and suitability for diverse photon-based technologies, making it an attractive candidate for future optoelectronic and photonic devices.15,30,76
The efficiency of a photocatalyst relies significantly on its light absorption capability, crucial for initiating photogenerated charge carriers within the material. Fig. 8(a), describes the absorbance (A) versus the wavelength (λ) of BaZrO3 in three radiation domains: UV (ultra-violet), Vis (visible) and NIR (near infrared). The absorption band is observed in the UV-region in the wavelength range of 200–800 nm.
Fig. 8(a) illustrates that BaZrO3 exhibits its primary absorption peak at 230 nm, attributed to band-to-band transition. Additionally, a band tail extending beyond 400 nm is evident, indicating the presence of disordered states, defect states, or oxygen vacancies within the compound. Such impurities or defect-state transitions typically manifest as band tails in semiconductor absorption spectra.6 The occurrence of absorption bands in the UV-VIS range indicates the capability of BaZrO3 to absorb UV and visible light. This characteristic renders them suitable for applications such as UV-VIS light absorption, the development of photovoltaic solar cells, and the creation of photocatalytic materials.77 Semiconductors in photovoltaic solar cells can capture energy from both UV and visible light, enabling the generation of electricity. In photocatalysis, these semiconductors can also promote chemical reactions upon exposure to either UV or visible light.78 The absorbance-wavelength spectra enabled the determination of an optical bandgap energy value that corresponds to the absorption band observed in the UV-Vis region. The determination of the bandgap energy for the BaZrO3 sample under study can be accomplished using Tauc's law31,32
| αhν = β(hν − Eg)n | (4) |
In this equation, ‘hν’ represents the photon energy of the substance and ‘β’ is a constant. In this particular scenario, two distinct optical transitions were identified: one with ‘n’ equal to 1/2, indicative of a direct transition type, and another with ‘n’ equal to 2, signifying an indirect transition. The determination of the band gap energy can be accomplished by applying the Tauc expression provided below.
| (αhν)1/n = β(hν − Eg) | (5) |
Fig. 8(b) illustrates the plots of (αhν)1/2 and (αhν)2 as a function of varying photon energy (hν) for the BaZrO3 compound. By linearly extrapolating the curves shown in Fig. 8(b) to zero hν, the determined values for the indirect and direct band gap energies are found to be (Eg)indirect = 3.0827 eV and (Eg)Direct = 3.846 eV, respectively. The observed band gap energy (Eg) for the sample produced in this study is lower than that reported in previous research. This reduction in the band gap is attributed to the high sintering temperature and is indicative of the quantum confinement effect.79 Moreover, upon comparing our findings with theoretical values, we find a good match, confirming that the band gap energy has indeed decreased. Reducing the bandgap value can boost the rate of electron–hole pair generation on the surface of the nanocatalyst, leading to an overall improvement in photocatalytic activity.21,22
The determination of the refractive index in BaZrO3 is accomplished using a contemporary empirical linear relationship between the energy band gap and refractive index, as proposed by Paswan80et al.
| n = 4.084 − 0.62Eg | (6) |
Subsequently, Fresnel's equation is utilized to compute the corresponding reflectance value.
![]() | (7) |
The determined value for ‘n’ in the case of BaZrO3 is 2.17, while the computed value for ‘R’ stands at 0.1375.
| S. No. | Photocatalyst | Illumination | Synthesis method | Contaminant | Results | Ref. |
|---|---|---|---|---|---|---|
| 1. | BaZrO3 | UV radiation | Green synthesis | CR dye | Degradation efficiency, 84.1% in 90 min, k = 0.0175 min−1 | Kayathiri et al., (2022)9 |
| 2. | BaZrO3:W 15% | UV–A | Hydrothermal synthesis | Levofloxacin | Degradation efficiency 93.4% and k = 1.27 × 10−2 min−1 | Gulen et al. (2021)64 |
| 3. | BaZrO3:W 5% | Visible light | Hydrothermal synthesis | Tetracycline | Degradation efficiency 94.9% and k = 1.01 × 10−2 min−1 | Gulen et al. (2021)64 |
| 4. | BaZrO3:Dy3+ | UV illumination | Hydrothermal synthesis | Methylene Blue | Degradation efficiency 78.66%, in 180 min and k = 0.015 min−1 | Aarti et al. (2024)84 |
| 5. | 3% carbon dots modified BaZrO3 | UV radiation | Facile carbonation process via the hydrothermal route | Methylene Blue | Degradation efficiency ∼90% | Patra et al. (2018)6 |
The photocatalytic activity of the synthesized catalyst was examined by assessing its ability to degrade rhodamine B under visible light irradiation (λ = 400 nm) using a 150 W Xe lamp. Under visible light irradiation, the color of the RhB/BaZrO3 suspension changes and the absorption gradually decreases, indicating that the ethyl groups were removed and thus, RhB was degraded. When exposed to visible light, BaZrO3 becomes activated and generates photo-induced electron–hole (e−/h+) pairs. Following this, photo-induced electrons rapidly migrate from BaZrO3 to RhB. As a widely recognized phenomenon, these photo-induced electrons efficiently catalyze the reduction of O2 molecules adsorbed on the surface of RhB/BaZrO3, yielding
radicals that play a pivotal role as key active species in the degradation process.86 In addition, the photo-induced h+ can oxidize RhB or react with H2O to generate OH* radicals. The generated OH˙ and
radicals can then oxidize RhB. The photo-degradation mechanism of RhB by BaZrO3 can be described by the following reactions:87
| BaZrO3 + hν → eCB−(BaZrO3) + h+VB(BaZrO3) | (8) |
| h+VB(BaZrO3) + H2O → OH* + H+ | (9) |
![]() | (10) |
![]() | (11) |
![]() | (12) |
| OH* + RhB → Degradation Products → CO2 + H2O | (13) |
| h+ + e− → (e−,h+) (negligible recombination) | (14) |
Fig. 9(a) displays the temporal UV-vis spectral changes of RhB aqueous solution during photocatalytic degradation reactions. Under visible light irradiation (λ = 400 nm) in the presence of BaZrO3, the primary absorbance peaking at 552 nm significantly decreased with irradiation time, resulting in approximately 35 to 38% degradation after 40 minutes of irradiation, as depicted in Fig. 9(a). The efficiencies of the photocatalytic degradation under visible light irradiation are illustrated in Fig. 9(b), where C represents the absorption of RhB at a wavelength of 552 nm, and C0 signifies the absorption after adsorption equilibrium on BaZrO3 before irradiation.
![]() | ||
| Fig. 9 (a) Degradation absorbance spectra of RhB dye using BaZrO3 nanoparticles, and (b) and (c) degradation rate. (d) Efficiency of dye for degradation under visible light. | ||
The BaZrO3 photocatalyst undergoes energy absorption upon illumination with light. Upon reaching or surpassing the energy band-gap of BaZrO3, the transfer of electrons (e−) occurs from the valence band to the conduction band. The transitions lead to the creation of holes (h+) in the valence band, and the resulting electron–hole pairs (e− and h+) generated by the photo-excitation process then migrate towards the surface of BaZrO3. However, the energy transfer induced by the photo-excitation is directed towards the adsorbed species, where the electrons are responsible for reducing the oxygen (O2) molecule to the oxygen-radicals (
), which are further converted into hydroxyl-radicals (OH*). Meanwhile, the holes produced by the photo-excitation process oxidize the hydroxyl (H2O) molecule to generate the hydroxyl-radicals (OH*).88 The resulting hydroxyl-radicals (OH*) are effective at decomposing RhB. The value of k is reported to be ∼0.0123 min−1, as shown in Fig. 9(c). The degradation efficiency of BaZrO3 reached ∼36.41% when exposed to UV-Visible light for a duration of ∼40 minutes, as recorded in Fig. 9(d).
From Fig. 10(a), it is seen that the minimum conduction band of BaZrO3 mainly consists of the Zr 4d orbital and a minor hybridization of Ba 4d orbital in the energy region from 4 to 6 eV. The maximum valence band consists of the hybridization of O 2p and Zr 4p orbitals in the energy region from −0.2044 eV to −4.0680 eV. Indeed, the s and p states of the zirconium atom, as well as the s state of the barium atom, exert a partial influence on these valence bands, and their presence can be observed. At energy levels surpassing the Fermi energy, which corresponds to the conduction band, there exist vacant states, including the unoccupied 4d states of the zirconium atom and the 6s and 5d states of the barium atom.91,92
The symmetrical pattern of density of the states indicates the existence of non-magnetism in BaZrO3. As shown in Fig. 10(b), the conduction band of BaZrO3 is mainly composed of Zr 4d states while the valence band is strongly dominated by O 2p.
In order to investigate the contribution of various atomic orbitals (s, p, and d orbitals) of BaZrO3, the projected density of states (PDOS) ranging from −5 eV below the top of the VB to 10 eV above the top of the VB band has been computed and illustrated in Fig. S5.† It represents the main orbital that influences the gap state. In the VB main role is played by O 2p (px, py, and pz) orbitals within a range of −0.3 eV to −4.3 eV due to the admixture of Zr (4d) and Ba (5p, 6s) states just below the Fermi level, which can be seen in Fig. S5(a and b).† This is expected due to the large electronegativity of oxygen (3.44 eV) as compared to Ba (0.89 eV) and Zr (1.33) (Pauling scale). It is also to be noted that the formation of the conduction band maximum (CBM) is dominated by the d-orbital contribution of the Zr atoms except for a small contribution of the p-orbital of O atoms (especially pz orbital). To explore further the orbital contribution to the conduction bands, PDOS for d-orbitals of Zr atoms have also been analyzed and are presented in Fig. S5(b).† The conduction band minima is mainly contributed by the dxz orbital of Zr(4d) atom with minor contribution from dxy and dyz orbitals within the energy range from 2.86 to 8.17 eV.
Significantly, our results are in agreement with previously reported data in the scientific literature.101 The Bader analysis underscores a greater covalent nature in the Zr–O bonds as opposed to the Ba–O bonds. This observation becomes apparent when considering that the effective Bader charge of Ba represents 76.145% of its ionic threshold, while Zr's effective Bader charge falls significantly shorter at 62.38% of its ionic limit. Hence, the Bader analysis highlights that within BaZrO3, the Zr–O bond demonstrates a reduced ionic quality and a heightened covalent aspect when compared to the Ba–O bond.
![]() | ||
| Fig. 11 (a) Photoluminescence mechanism. (b) Photo luminescence spectra at the excitation wavelength λexc = 400 nm. (c). CIE diagram of BaZrO3 nanoparticles. | ||
The room temperature photoluminescence spectra of BaZrO3 nanoparticles, synthesized through a straightforward one-step flash combustion method, employing an excitation wavelength of 400 nm is showcased in Fig. 11(b). When subjected to this 400 nm excitation, the spectra manifest a prominent and expansive range of violet-blue emissions. Specifically, the violet emission peaks are located at 420.57 nm and 429.90 nm, while the indigo emission peaks are discernible at 442.98 nm, 452.49 nm and 459.82 nm and the blue emission peaks are discernible at 470.6 nm, 484.32 nm and 493.60 nm. The peaks at 502.63 nm, 521.17 nm and 536.96 nm correspond to the Green region.
The photoluminescence (PL) emission spectra depicted in Fig. 11(b) demonstrate a continuous spectrum of emissions, owing to the involvement of multiple components. To assess each component individually, it is imperative to deconvolute the spectra. Street and Bevingt proposed that these profiles could be separated using a Lorentzian line shape function. In our current study, we employed the Gaussian line shape function to deconvolute the PL spectra, effectively utilizing the Lorentzian line shape to fit the emission peaks. Emission peaks at 420.57 nm (2.94 eV), 429.90 nm (2.88 eV), 442.98 nm (2.79 eV), 452.49 nm (2.74 eV), 459.82 nm (2.69 eV), 470.60 nm (2.63 eV), 484.32 nm (2.56 eV), 493.60 (2.51 eV), 502.63 nm (521.17 eV) and 536.96 nm (2.30 eV) nm were observed. The presence of these emission bands signifies the existence of seven strong and distinct electronic transitions within the visible spectrum, spanning from violet to yellow wavelengths.19,20 Nevertheless, it is worth noting that the most prominent emission peak, which appears at approximately 420.57 nm (equivalent to 2.94 eV), displays the highest intensity among all the observed emissions. This emission peak suggests that BaZrO3 exhibits heightened activity in the violet light region when subjected to visible light irradiation.90,91 The radiative defect peaks are observed at 420.57 and 429.90 nm. Size-dependent excitonic transition is responsible for the emission peak at 470.60 nm.76 The peaks at 502.63, 521.17, and 536.96 nm might have been originated from vacancies or point defects which are either extrinsic or intrinsic that form recombination centers. The presence of recombination sites and defects can also play a role in influencing the process.30,101
The Commission International de I’ Eclairage (CIE) chromaticity coordinates are crucial factors for evaluating the luminescence properties of phosphors.31 The CIE 1931 x–y chromaticity diagram of BaZrO3 nanophosphors were presented in Fig. 11(c). According to PL spectra, the CIE chromaticity coordinates (x, y) of BaZrO3 are (0.18324, 0.19117). The red star in Fig. 11(c) represented the location of the CIE chromaticity coordinate of BaZrO3 under excitation wavelength 400 nm. These coordinates are situated in the violet-blue region, indicating the dominant color of the emitted light, which further verifies the potential application of BaZrO3 nanophosphors in the production of intense violet-bluish LEDs.
m (221) space group with a crystallite size of 70.29 nm. Charge density plots revealed a charge transfer mechanism indicating the more ionic nature of the Ba–O bond compared to that of Zr–O. The surface morphology showed uniform particle dispersion with an average size of 45.31 nm. Negative phonon frequencies suggested potential structural phase transitions, and FTIR supported sample purity. Raman spectroscopy indicated second-order scattering, while XPS provided insights into surface compositions and oxidation states. UV-Vis spectroscopy showed a reduced bandgap energy of 3.08 eV, enhancing photocatalytic potential, with a degradation efficiency of 36.41% for rhodamine B under visible light. Photo-luminescence spectra displayed intense violet emission at 420.57 nm. Combining DFT simulations with extensive experimentation, this study highlights BaZrO3's tailored properties, and promising applications in photocatalysis and violet-bluish LEDs. Further research could amplify BaZrO3's capabilities.
Our study presents a novel synthesis method for BaZrO3, enabling precise control over particle size and morphology while addressing scalability challenges. Using advanced techniques like UV-spectroscopy and DFT analysis, we demonstrated the ability to fine-tune the bandgap, significantly enhancing BaZrO3's potential applications in electronics and catalysis.
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4nr00517a VK Current Address- Surface Science Laboratory, Department of Materials and Earth Sciences, Technical University of Darmstadt, Otto-Berndt-Straße 3, 64287 Darmstadt, Germany. E-mail: vkumar@surface.tu-darmstadt.de |
| This journal is © The Royal Society of Chemistry 2024 |