Amidst the pressing demand for carbon neutrality and clean energy policies, the electrocatalytic urea oxidation reaction (UOR) has gained attention as an efficient and environmentally friendly energy conversion pathway. High-valence/content two-dimensional (2D) nickel-based ABO3 perovskite oxides, particularly LaNiO3, are highlighted for their elevated intrinsic catalytic activity and rich electronic configuration advantages. To enhance the intrinsically limited conductivity of LaNiO3, a modified strategy involving B-site substitution can be used to construct a solid solution structure, significantly improving the electronic configuration. However, as Ni is the primary active site for the UOR, substituting the B-site will create a trade-off between enhancing electron migration and decreasing active site content. Specifically, conventional synthesis methods with a slow-entropy-change pose challenges in precise control over atomic ratios and 2D structure design, hindering elucidation of the impact mechanism of the electronic configuration on UOR performance. Herein, we utilized the microwave-pulse method for rapid synthesis of highly tunable 2D porous nickel-enriched LaMnxNi1−xO3 perovskite. Leveraging transient high-temperature and high-energy conditions, we achieved rapid one-step equilibrium between 2D porous structure design and precise control of solid solution atomic ratios. This strategy allows for the controlled synthesis of 2D nickel-enriched solid solutions with excellent conductivity and UOR activity, while effectively avoiding the generation of by-products, providing a detailed analysis of the UOR activity mechanism dependent on distinct electronic configurations. The synthesized LaMn0.2Ni0.8O3 structure exhibits optimal UOR performance. This strategy provides a new avenue for the design of more unique structured nickel-based solid solutions and the investigation of their structure–performance relationships in the electrocatalytic UOR.
Fig. 1 (a) The process of a nickel-based catalyst reaction in the UOR. (b) LaMnxNi1−xO3 (x = 0, 0.2, 0.4, 0.6, 0.8) crystal structure diagram. |
To successfully engineer a 2D structure for LaNiO3 (LNO) while elucidating the impact mechanism of Ni content on its UOR activity through a clear understanding of the optimal electronic configuration in B-site substitution, poses a challenge of balancing the thermodynamics of 2D oriented growth with the kinetics of transiently controlling the Ni atomic ratio. Actually, there are currently various methods available for the successful preparation of nickel-based oxide solid solutions, which represent a type of alloy phase material capable of effectively integrating the target elements with the matrix elements, maintaining the homogeneous crystal structure characteristics of the matrix elements. This is a strategy capable of utilizing a targeted atomic ratio to influence the electronic configuration of the parent material, aiding in deciphering its corresponding impact mechanism on electrocatalytic activity.28 For example, Rao et al. synthesized Mn0.1Ni0.9O nanoparticles by solution combustion after high temperature calcination for half an hour, which significantly improved their electrocatalytic activity in the OER.29,30 Additionally, Wang et al. successfully synthesized stable multi-metal NiCoFe-O@NF nanoparticles using a prolonged hydrothermal method, inducing enriched Co2+ and Ni3+ configurations, thereby adjusting the electronic structure and demonstrating exceptional dual-catalytic activity for both the hydrogen evolution reaction and OER under alkaline conditions.31 Although conventional synthesis methods involving slow-entropy-change processes can effectively enhance the bulk/interface catalytic activity of nickel-based oxides through solid solution design, they often exhibit typical nanoparticle structures and relatively arbitrary atomic ratios, making it challenging to simultaneously control 2D selective oriented growth and the specific atomic ratio of the target elements. Moreover, undesired by-products and impurities may also be generated due to inappropriate precursor ratios. Thus, it is imperative to seek a method for precise design of the Ni atomic ratio in 2D LaMnxNi1−xO3 solid solution through B-site substitution.
Over the past decade, advanced non-liquid-phase microwave technology has been able to exploit mechanisms such as dipolar loss, conduction loss, and magnetic loss to rapidly construct numerous unique nanostructures from both thermodynamic and kinetic perspectives. For instance, Sun et al. achieved rapid synthesis of high-quality graphene within 200 seconds using the microwave method,32 while Wan et al. demonstrated the 2D structural evolution of TMCs over 3 times of microwave pulse approach.33 Subsequently, precise control over metal element doping, especially the successful introduction of high atomic ratios, was accomplished using the microwave discharge method.34 Considering the involvement of Ni as the primary active site for the UOR, this suggests a conceptual and feasible approach to construct nickel-rich 2D LaMnxNi1−xO3 solid solutions using microwave technology.
Herein, taking manganese (Mn) as an example with rich oxidation states and abundant sources, we successfully prepared highly tunable 2D porous LaMnxNi1−xO3 perovskite using a microwave-pulse method. By leveraging the thermodynamic and kinetic advantages of microwave transient high temperature and high energy, a rapid one-step achievement of balanced design for 2D porous structures and atomic ratio precision control can be realized. This strategy can effectively avoid the generation of by-products, precisely regulating the Ni–Mn atomic ratio to achieve the optimal coupling of conductivity and UOR catalytic activity. Subsequently, the mechanisms underlying the electronic configuration-dependent UOR activity are further elucidated. The synthesized LaMn0.2Ni0.8O3 structure exhibits an optimal electrocatalytic UOR performance (a low potential of 1.27 V at a current density of 10 mA cm−2 and a low Tafel value of 44.6 mV dec−1), highlighting the synergistic effect of its conductivity and nickel active site content. This strategy provides a novel approach for the precise design of more 2D nickel-based UOR electrocatalysts and mechanistic studies of structure–performance relationships.
The electronic configurations of Ni and Mn, which differ in their d orbital electron arrangements, are [Ar]3d84s2 for Ni and [Ar]3d54s2 for Mn. The substitution of Ni cations at the B-site with Mn leads to interactions between their electrons, potentially enhancing the structure and properties (Fig. 3a). To investigate the impact of Mn substitution at the B-site on the crystal structure of 2D porous LNO perovskites, XRD analysis was conducted on LNO, LNMO-0.2, LNMO-0.4, LNMO-0.6, and LNMO-0.8 samples to examine their phases and crystal structures. Rietveld refinement using GSAS software and the EXPGUI interface further determined the space groups and lattice parameters of these samples (Fig. 3b), revealing that LaMnxNi1−xO3 (x = 0, 0.2, 0.4, 0.6, 0.8) possesses a rhombohedral perovskite structure (space group: Rc). Due to the larger ionic radius of Mn3+ compared to Ni3+, the lattice parameters of LNMO changed. From Fig. S7†, it is evident that the metal–oxygen bonding stretching vibration occurs around a wavenumber of 600 nm−1. A slight shift of the main diffraction peak at 32.9° for the LNO (110) plane towards lower angles indicated an expansion of the lattice spacing (Fig. 3c). This expansion can be attributed to the changes in lattice parameters due to the variation in ionic radii between Mn3+ (0.66 Å) and Ni3+ (0.63 Å) cations. Fig. 3d shows that the Ni–O bond length is increasing, from 1.97 Å to 2.04 Å. Similarly, the Mn–O bond length increases from 1.98 Å to 2.04 Å. Fig. 3e presents the changes in bond angles; the angle between O–Mn1–O and O–Ni2–O increases from 90.04° to 93.34°. Meanwhile, the angle between O–Mn2–O and O–Ni1–O decreases from 88.45° to 86.66°. This further confirms the substitution of Mn for Ni at the B-site. Fig. 3f shows the refined error values for different samples, which can be considered as strong evidence of the successful preparation of a series of LNMO samples and the significant substitution of Mn for Ni at the B-site.
To better understand the electronic structure of solid solutions with varying Mn/Ni ratios, X-ray photoelectron spectroscopy (XPS) was used to characterize the valence states of the constituent elements in the LNMO-x samples. The full XPS spectrum of LNMO-x revealed the presence of La, Mn, Ni, and O elements (Fig. S8†). The Ni 2p orbitals partially overlapped with the La 3d orbitals, with the characteristic peak at 851 eV attributed to La 3d3/2. The Ni 2p3/2 orbitals were divided into Ni3+ and Ni2+, with the peak at 852.8 eV corresponding to the satellite peak of Ni 2p3/2. The Mn 2p orbital data showed that 642.7 eV and 654.4 eV correspond to Mn 2p3/2 and Mn 2p1/2, respectively. The Mn 2p3/2 orbitals were divided into Mn4+ and Mn3+ peaks, resulting in a strong Mn–O bond.42 In the rate-determining step of the OER, a stronger Mn–O bond can also promote charge transfer between surface Mn ions and oxygen intermediates (such as O22− and O2−) (Fig. S9†).43 If the formation potential of the active phase is too high, the OER might compete with the UOR, thereby reducing the selectivity of the UOR.44,45 In alkaline media, surface Ni2+ ions adsorb hydroxide ions to form Ni(OH)2, which can be oxidized to NiOOH at higher potentials. NiOOH is commonly considered as the active site for the UOR, making the intrinsic content of Ni3+ a reasonable indicator of UOR activity.46 Therefore, maintaining a high concentration of Ni3+ is crucial for UOR activity. We further analyzed the content ratio of Ni and Mn elements. As shown in Fig. 4a, we found that the content of Ni3+ in LNMO-0.2 was 65.03%, and that of Ni was 34.97%, which was an increase compared to 58.8% and 41.2% in LNO. However, with further introduction of Mn, the Ni3+/Ni2+ ratio decreased. Similarly, Fig. 4b shows the trend of Mn4+/Mn3+ content variation. As shown by the characteristic peaks of the O 1s orbital, the peak at 529.1 eV corresponds to lattice oxygen, 531.9 eV to surface adsorbed oxygen and hydroxyl groups, and 534.4 eV to surface adsorbed water molecules.47 The strong peak of surface adsorbed oxygen and hydroxyl groups is likely related to the generation of oxygen vacancies (Fig. S10†). To more accurately characterize the variation in oxygen vacancy (Ov) content, electron paramagnetic resonance (EPR) analysis was performed on LNO and LNMO-0.2. As shown in Fig. S11†, under the condition of g = 2.002, the EPR signal intensity of LNMO-0.2 was stronger than that of LNO (indicating a higher concentration of unpaired electrons/Ov), suggesting that the introduction of Mn effectively increases the Ov concentration.48Fig. 4c displays the relationship between Ni3+/Ni2+ and oxygen vacancies, revealing a positive correlation between the concentration of oxygen vacancies and the Ni3+/Ni2+ ratio. According to the principle proposed by Shao-Horn, an optimized eg filling near 1.2 should be an effective strategy for developing transition metal oxides as efficient catalysts, as an eg electron ratio close to 1.2 enhances the hybridization between the 3d–eg orbitals of the transition metal and the 2p orbitals of oxygen.49–51Based on this, the eg orbital filling numbers for LaMnxNi1−xO3 (x = 0, 0.2, 0.4, 0.6, 0.8) were calculated to be 0.597, 1.150, 1.002, 0.850, and 0.696, respectively (Fig. 4d). In nickel ions (Ni2+), the high occupancy of the eg orbitals, as manifested in the t2g6eg2 configuration, results in a strong binding affinity with reaction intermediates, thereby impeding the desorption of gaseous products. However, an eg electron filling number approaching 1.2 can significantly enhance the adsorption and desorption processes of these intermediates, which contributes to improving the catalysis of the UOR.9 Increased oxygen vacancies often lead to enhanced electrical conductivity, and variations in the bandgap width typically indicate changes in conductivity. The UV-vis absorption spectra of LNMO-x showed that the measured bandgap width for LNMO-0.2 was 1.83 eV, a decrease of 0.42 eV compared to the bandgap width of LNO (2.25 eV) (Fig. 4e). Bandgap information for other samples is presented in Fig. S12.†Fig. 4f provides a schematic representation of the changes in the bandgap width. The observed reduction in the bandgap width suggests enhanced conductivity, which is beneficial for rapid electron transfer in materials such as electrocatalysts. These results indicate that the partial substitution of Mn at the B-site in LNO affects its electron transfer properties, enhancing its conductivity. Introducing more oxygen defects in the structure affects the proportion of Ni3+ at the B-site, thereby increasing the number of reactive sites. Overall, the LNMO-0.2 structure, characterized by a significant presence of oxygen vacancies and a high Ni3+ content, is the result of a balanced approach to 2D porous structure design and precise control of the atomic ratio in solid solutions. Therefore, LNMO-0.2 holds promise as a highly active material for electrocatalytic UOR applications.
To assess the impact of partial Mn substitution at the B-site on the UOR activity of LNO, comprehensive electrochemical characterization of the synthesized electrocatalysts was conducted using a standard three-electrode setup in a 1 M KOH + 0.33 M urea electrolyte. Fig. 5a presents the linear sweep voltammetry (LSV) polarization curves for LNO and LNMO-0.6, and it was observed that the UOR possesses a lower thermodynamic potential compared to the OER, indicating more rapid reaction kinetics for the UOR. However, beyond a potential of 1.4 V, a competitive relationship between the UOR and OER may emerge. Consequently, with the further incorporation of Mn, there is a likelihood of a decrease in the catalytic activity of the UOR. Fig. 5b shows the LSV polarization curves for LaMnxNi1−xO3 (x = 0, 0.2, 0.4, 0.6, 0.8). Notably, LNMO-0.2 exhibited a lower potential at a current density of 10 mA cm−2 (1.275 V) compared to LNO (1.434 V), LNMO-0.4 (1.326 V), LNMO-0.6 (1.374 V), and LNMO-0.8 (1.413 V), indicating the highest UOR activity among the perovskite oxide electrocatalysts studied. Moreover, the Tafel slope values of the samples showed significant differences (Fig. 5c). The Tafel slope of the LNMO-0.2 sample was significantly lower at 44.6 mV dec−1 compared to that of LNO (98.1 mV dec−1), LNMO-0.4 (58.0 mV dec−1), LNMO-0.6 (66.7 mV dec−1), and LNMO-0.8 (89.2 mV dec−1). This observation strongly suggests enhanced reaction kinetics in the UOR process for the LNMO-0.2 sample, indicating its potential as a superior electrocatalyst with improved electrocatalytic performance. A significant decrease in the Tafel slope indicates accelerated reaction kinetics, which may imply a change in the rate-determining step. The observed reduction in the Tafel slope can be attributed to the favourable adsorption of intermediates, resulting from electronic modulation caused by the presence of Mn4+. The overpotentials and Tafel values of all samples are presented in Fig. 5d. LNMO-0.2 showed the lowest potential and Tafel slope, indicating excellent UOR activity.
To gain further insight into the intrinsic activity of the catalysts, the electrochemical surface area (ECSA) was evaluated by measuring the electrochemical double layer capacitance (Cdl) within a scan range of 1.13–1.23 V (Fig. S13†). As shown in Fig. 5e, the calculated Cdl values for LNO, LNMO-0.2, LNMO-0.4, LNMO-0.6, and LNMO-0.8 were estimated to be 5.48, 9.16, 8.59, 7.56, and 6.78 mF cm−2, respectively. These results indicate that the high UOR current density obtained with the LNMO-0.2 electrode is the result of a balance between the precise introduction of Mn and the construction of 2D structure. To evaluate the UOR kinetics of the perovskite oxide electrocatalysts, electrochemical impedance spectroscopy (EIS) analysis was performed on all samples at an open-circuit potential with an AC amplitude of 10 mV, in a frequency range of 100 kHz to 0.01 Hz. Nyquist plots are shown in Fig. 5f. Compared to other electrocatalysts, LNMO-0.2 exhibited the smallest radius, indicating the lowest charge transfer resistance (Rct). The Rct values for LNO, LNMO-0.2, LNMO-0.4, LNMO-0.6, and LNMO-0.8 were 8.53, 5.98, 7.44, 8.03, and 8.19 Ω, respectively. The excellent characteristics of LNMO-0.2, with fast charge transfer and low resistance, are well-aligned with the Tafel slope results, further supporting its potential as a highly effective electrocatalyst for the UOR. The response in the low-frequency region of the Nyquist plots for LNMO-0.4, LNMO-0.6, and LNMO-0.8 showed differences, with the diffusion process in LNMO electrodes evidently accelerating. These results suggest that the substitution of Mn significantly enhances the reaction kinetics, thereby improving the UOR performance. This collectively confirms that substituting Mn at the B-site in LNO perovskite oxides effectively improves the conductivity during the OER process and enhances charge transfer capabilities. The exceptional UOR electrocatalytic activity of LNMO-0.2 surpasses that of many catalysts (Fig. 5g and Table S2†).2,52–65 Electrocatalysis requires the stability of electrodes, as commercial electrodes must maintain a stable potential over extended periods. As shown in Fig. 5h, we assessed the long-term electrochemical stability of LNMO-0.2 using chronoamperometry tests at 50 mA cm−2. The durability assessment was conducted at a constant current density of 50 mA cm−2. The results demonstrated significant stability of the potential, with negligible decay even after approximately 30 hours of continuous operation under alkaline conditions. In the accelerated durability assessment (Fig. S14†), LNMO-0.2 consistently exhibited outstanding UOR performance, even after enduring a 30 hour durability test at a scan rate of 10 mV s−1. Notably, the powder XRD spectrum of LNMO-0.2 remained largely unchanged after the stability test (Fig. S15†). Post-durability test SEM images of LNMO-0.2 showed that the 2D porous morphology was maintained with no significant aggregation observed (Fig. S16†). We employ EDS to analyze the elemental composition of electrode materials after testing. This will help us confirm that the distribution and concentration of La, Mn, and O elements in the material remain essentially unchanged over prolonged operation, while the Ni content decreases. This demonstrates the role of Ni as an active site in the catalyst (Fig. S17†).
HRTEM will allow us to observe the microstructure of the catalyst at high resolution after stability testing. We found that the crystal structure of the catalyst remains stable throughout long-term electrochemical reactions, with no particle agglomeration or morphological changes (Fig. S18†).
XPS analysis will be utilized to assess changes in the surface chemical state of the catalyst, especially the chemical environment and valence changes of Ni active sites. The observed decrease in signal intensity of Ni, with the ratio remaining fundamentally unchanged, indicates that the redox reactions occurring during the electrochemical process are reversible (Fig. S19†). This indicates negligible changes in the surface composition of the sample after the durability test. This 2D porous LNMO-0.2, with partial Mn substitution at the B-site, achieves a balance between 2D porous structure design and precise control of the atomic ratio in solid solutions. It facilitates electron transfer in electrocatalytic processes and exhibits stable UOR performance.
In the field of electrocatalysis, the d band center theory is one of the most representative descriptors. We have utilized descriptors derived from density functional theory (DFT) and molecular orbital theory to interpret the performance of a series of LNMO catalysts. To investigate the impact of Ni introduction on the electronic configuration of LMO, DFT calculations were employed to study the electronic configurations of LMO, LNMO-0.2, LNMO-0.4, LNMO-0.6, and LNMO-0.8. Their projected density of states (PDOS) is displayed in Fig. 6a. The valence band states below the Fermi level (Ef) are primarily derived from Mn 3d and O 2p orbitals. As the concentration of Ni increases, the overlap between the partial DOS of occupied and unoccupied 2p orbitals and the partial DOS of Mn 3d promotes the hybridization of Ni 3d with O 2p. This hybridization can lower the charge transfer barrier between O 2p and Ni 3d, thereby enhancing the kinetics of oxygen electrode reactions.66
As shown in Fig. 6b and c, the d band center of Mn is far from the Fermi level, while the d band center of Ni shows a shifting process relative to the Fermi level. This shift in the d band center of Ni, as a result of varying Ni concentrations, indicates changes in the electronic structure that can significantly affect the catalytic activity. The proximity of the d-band center to the Fermi level is a key factor in determining the reactivity of transition metal catalysts, as it influences the extent of electronic interaction between the catalyst and reactants.67,68 In summary, the DFT analysis suggests that the introduction of Mn into the LNO structure modifies the electronic interactions, particularly through the hybridization of Ni 3d and O 2p orbitals, which is conducive to improved catalytic activity for the UOR. This finding is consistent with the observed enhanced UOR activity in LNMO catalysts, particularly LNMO-0.2, which displayed the highest activity among the samples studied. From the perspective of molecular orbital theory, when adsorbate molecules approach the metal surface, their orbitals interact with the metal's s and d orbitals, leading to energy level splitting. The resulting bonding orbitals are lower in energy and more stable than the original orbitals, while antibonding orbitals are higher in energy and less stable. The more electrons that fill the antibonding orbitals, the less stable the structure becomes, weakening the bond strength of the intermediates (Fig. 6d).69,70 Upon the interaction between the adsorption energy levels and the continuous energy levels, its energy between bonding orbitals and antibonding orbitals undergoes a certain degree of broadening. The width of this broadening represents the interaction strength between the metal's d orbitals and the adsorbate's p orbitals; the stronger the interaction, the wider the d band broadening. When the broadening narrows while the Fermi level remains constant, the d band center rises. Consequently, the fewer the electrons in the antibonding orbitals, the greater the adsorption energy.71 To further clarify the key factors of the d-band in LNMO, we calculated the d-band centers of Ni and Mn for all samples. In the UOR, the strong binding of Ni3+ active sites with *COO intermediates can lead to poisoning effects. The thermodynamic energy of this reaction is substantial, resulting in lower catalyst activity. Therefore, we aim to reduce the adsorption energy at the Ni active sites. As shown in Fig. 6e, the d band center of Ni exhibits a volcanic shape, decreasing from −1.69 eV to −2.70 eV and then increasing to −1.94 eV. This indicates a weakening of adsorption, which is favorable for the occurrence of the UOR. This also explains why LNMO-0.2 exhibits the best UOR activity. Since the OER competes with the UOR at high potentials, we aim to suppress the occurrence of the OER. According to Sabatier's principle, the binding between the catalyst and substrate should not be too strong or too weak, as this is detrimental to the catalytic reaction. Hence, we observe that Mn's d band center continuously rises, indicating stronger adsorption energy. This is increasingly favorable for the OER, where the rate-determining step is the initial adsorption of oxygen intermediates, inadvertently suppressing reactions. Therefore, by combining theoretical calculations, we have achieved a balance between the design of 2D porous structures and the precise control of the atomic ratio in solid solutions.
In the synthesis of 2D LNMO-x, 0.4 g glucose, 0.433 g La(NO3)3·6H2O, 0.291 g of Ni(NO3)2·6H2O, 0.251 g of Mn(NO3)2·4H2O, and 0.5 g NH4NO3 were ground thoroughly in a mortar. Then the mixture was transferred into a custom-made quartz tube (inner diameter of 12 mm, wall thickness of 2 mm) inside a microwave reaction unit. 2D porous LNMO-x can be obtained after heating for 15 min (heating with four pulses of microwaves) with a power of 900 W without any purification process. The samples synthesized by using microwave shock times of 1 min, 1.5 min and 10 min were named LNMO, LNMO-1.5 and LNMO-10, respectively.
After ultrasonication for one hour in an ice bath, the mixture formed a homogeneous ink. Subsequently, 5 μL of this catalyst ink was deposited onto a mirror-polished glassy carbon electrode. The mass loading of each electrode was precisely controlled at 1 mg cm−2. The reference electrode used was Hg/HgO (in 1 M KOH + 0.33 M urea), and the counter electrode was a platinum plate. Calibration of the reference electrode was performed according to: E(RHE) = E(Hg/HgO) + E(Hg/HgO vs. RHE) + 0.0592 pH. All scans were performed under an argon atmosphere.
Polarization curves were obtained at room temperature with a scan rate of 5 mV s−1. The electrochemical surface area (ECSA) was estimated from the double-layer capacitance (Cdl) of the samples. Cdl was determined by measuring the corresponding cyclic voltammetry (CV) curves within a specific potential window at different scan rates ranging from 2 to 20 mV s−1. The absolute sum of cathodic and anodic currents at 0.18 V vs. RHE at different scan rates was plotted, and half of the obtained slope was taken as the Cdl. Electrochemical impedance spectroscopy (EIS) was then conducted at various overpotentials, in a frequency range of 0.01 to 105 Hz and at an amplitude of 10 mV. The stability tests were conducted on an electrochemical workstation, utilizing a three-electrode system. Our two-dimensional porous, nickel-rich LaMnxNi1−xO3 solid solution material served as the working electrode, with an Hg/HgO electrode as the reference electrode and a platinum wire as the counter electrode. Tests were performed at room temperature, using a 1 M KOH + 0.33 M urea solution as the electrolyte.
For the stability tests, we employed constant potential (CP) electrolysis to assess the catalyst's stability. For CV tests, the scan rate was set at 50 mV s−1, with a scanning range from 1.13–1.23 V (vs. RHE). A total of 1000 cycles were conducted to evaluate the electrochemical stability of the material throughout the cycling process. For CP tests, electrolysis was performed at the material's optimized activity potential for at least 30 hours to assess its long-term stability.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4ta00235k |
‡ Equal contribution. |