Surjyakanta
Rana
and
Sreekantha B.
Jonnalagadda
*
School of Chemistry & Physics, College of Agriculture, Engineering & Science, University of KwaZulu-Natal, Durban, South Africa. E-mail: jonnalagaddas@ukzn.ac.za; Fax: +27 31 260 3091; Tel: +27 31 260 7325 ext. 3090
First published on 12th January 2017
We report a facile and environmentally friendly protocol for the synthesis of novel mono-dispersed Cu and Ni bimetallic alloy particles supported on fibrous anime functionalized graphene oxide (GO). In this protocol, we used the organic amine group to increase the binding capacity of supported metal particles. First GO was covalently functionalized by organic amine [N-(2 amino ethyl)-3-amino propyl trimethoxy silane i.e., (AAPTMS)] to form AAPTMS–GO and then metal ions were loaded on the surface of the AAPTMS–GO material. The metal particles supported on AAPTMS functionalized graphene oxide were named as Ni–AAPTMS–GO, Cu–AAPTMS–GO and Cu–Ni–AAPTMS–GO to reflect the metals loaded, and all were fully characterized by various techniques including XRD, SEM, FTIR, Raman spectra, TEM and HRTEM analysis. The 5% loaded with a 1:1 ratio of Cu:Ni of Cu(0)–Ni(0)–AAPTMS–GO showed superb efficiency in conversion of p-nitrophenol to p-aminophenol with 100% conversion and selectivity. Hydrogenation of cinnamaldehyde with the same catalyst gave 85% conversion and 59.8% selectivity towards cinnamal alcohol (COL) at 80 °C. The catalyst also showed good stability in recycling tests.
Primary drawback associated with unsupported catalysis is that metallic catalysts cannot be reusable for several catalytic runs. Whereas with supported heterogeneous catalysts, allow easy separation and reusability, which is an attractive advantage. Although some agglomeration of metal nanoparticles during catalytic runs is inevitable, a right choice of support will minimize such processes. The supports containing organic groups can greatly influence the activity and selectivity of the catalyst material. Due to the nontoxicity and high sorption capacities,15–18 carbon based nanomaterials have been widely used as inorganic support for catalyst materials. In material science, graphene oxides enjoy prime position among the other carbon based materials, due to their honey comb like structure and high surface area.19,20
Transition metal salts like Cu and Ni are less-expensive and readily available, relative to the most of noble metal salts, which are normally used as catalysts. Therefore, in the current study, we have constructed low-cost Cu–Ni bimetallic nano particles grafted on amine functionalized graphene oxide surface. The amine functionalized graphene oxide as support material possess high surface area, which enhances the catalytic activity as well as dispersion capacity. The functionalized amine with external binding capacity will provide additional active sites and also increase its reusability.
Nitro substituted hydrocarbons are generally toxic by nature and hard to be degraded in the environment.21 In addition, the conversion of aromatic nitro-compounds to aromatic amino compounds obeys with the demands of green chemistry. Further, hydrogenation of unsaturated aldehyde to alcohol with heterogeneous catalytic processes is always a challenge, since the hydrogenation of the CO bond, while keeping the CC intact is not thermodynamically favourable. Thus, the hydrogenation is of supreme significance in fine chemical synthesis and many efforts have been made to design appropriate solid catalysts. Prakash et al. have reported that Ni–Au/TiO2 and Ni–Ag/TiO2 gave better activity towards hydrogenation of unsaturated aldehyde compared to their single mono metallic like Ni/TiO2.22 Lin et al., have also reported that Ir–Ni/TiO2 catalyst showed higher activity and selectivity in hydrogenation of unsaturated aldehydes compared to heterogeneous monometallic catalysts.23
In this study we developed a novel catalyst material, Cu–Ni bimetallic functionalised graphene oxide nanocomposite and investigated its activity on two organic transformations. The efficacy of the different loading of Cu and Ni on the support for selective reduction of p-nitrophenol as well as hydrogenation of cinnamaldehyde were examined and role of temperature and solvents on the reactions were assessed.
Similar method was used for preparation of Cu–Ni bimetallic nanoparticles by using hydrazine. To the Cu and Ni containing solution of functionalized GO, 0.2 M hydrazine solution was added under stirring. Then the suspension was vigorously stirred at RT for 6 h. The suspension was washed with acetone and preserved toluene. Then, the final solid product was vacuum dried at 100 °C for overnight (Scheme 1).
The FT-IR spectra (4000–400) of (a) AAPTMS@GO, (b) Ni–AAPTMS@GO, (c) Cu–AAPTMS@GO, (d) (1:1) Cu–Ni–AAPTMS@GO, (e) (1:1) Cu(0)–Ni(0)–AAPTMS@GO, (f) (1:2) Cu(0)–Ni(0)–AAPTMS@GO, and (g) (2:1) Cu(0)–Ni(0)–AAPTMS@GO are shown in ESI Fig. S1.† All the samples showed peaks at 3400 cm−1 and 1740 cm−1 due to O–H stretching, CO stretching of –COOH. The peaks at 1385 cm−1 and 1100 cm−1 also correspond to O–H vibration of C–OH groups and epoxy group vibration.31 The covalent functionalization of organic amine proceeds through two steps. In the first step, trialkoxy groups of silane generate –Si–OH groups by hydrolysis. Then the second step, the reaction between –Si–OH group of organo silane and –C–OH group of graphene oxide, covalently linked to the graphene surface through –Si–O–C– bond. In the FTIR spectra, the peak at 686 cm−1 is due to stretching vibrations of Si–O–C.32 The peaks at 3371 cm−1 and 1638 cm−1 corresponding to N–H stretching and NH2 bending mode of free NH2 groups due to the organic amine modification. These peaks give direct evidence to the successful silylation of the GO materials.
The Raman spectra of AAPTMS@GO (a), Cu–AAPTMS@GO (b), Ni–AAPTMS@GO (c), (1:1) Cu–Ni–AAPTMS@GO (d) and (1:1) Cu(0)–Ni(0)–AAPTMS@GO (e) are shown in ESI Fig. S2.† All the five samples showed similar characteristic D and G bands. In GO, the band at 1350 cm−1 corresponds to disorder in the sp2-hybridized carbon atoms in graphene oxide sheets from D-band, and 1590 cm−1 represents the σ-sp2 bonded C-atoms from G band of Raman spectra.31 After metal modification, the both D and G-band moved nearer to higher wave number, which may be due to the progressively increased compressive local stress caused by molecule intercalation as shown in ESI Fig. S2(a–e).†
X-ray photo electron spectroscopy give the information about the binding energy of Cu 2p and Ni 2p in (1:1) Cu(0)–Ni(0)–AAPTMS@GO catalyst in Fig. 2. The binding energy of Cu 2p3/2 and Cu 2p1/2 are 932.3 eV and 952.12 eV respectively. The binding energy of Cu 2p3/2 was ∼0.5 eV lower than that in the metallic state of Cu. The binding energy of Ni 2p3/2 and Ni 2p1/2 are 853.5 eV and 873.3 eV respectively, which was ∼0.5 eV higher than that in the metallic state of Ni catalyst.33 The shifting of binding energies of Cu 2p3/2 and Ni 2p3/2 confirm the formation of alloy nanoparticles between Cu and Ni and also interaction between metallic alloy and support surface.
TEM images of AAPTMS@GO (a), Cu–AAPTMS@GO (b), (1:1) Cu–Ni–AAPTMS@GO (c), (1:1) Cu(0)–Ni(0)–AAPTMS@GO (d), (1:2) Cu(0)–Ni(0)–AAPTMS@GO (e) and (2:1) Cu(0)–Ni(0)–AAPTMS@GO (f) samples, facilitate to examine the morphologies of the synthesized materials are shown in Fig. 3. The pure graphene oxide is composed of very thin sheets.28 After functionalization silane creates defects in the graphene oxide sheets, this morphology changes due to presence of organic solvents. The solvent appears to soften the severe attack of organic amine groups on GO surface and hinders breaking down of big sheets to smaller ones as shown in Fig. 3(a). Fig. 3(b) displays the only single metal particles, but in Fig. 3(c) displays the different phase of complex morphology of both bimetallic particles are formed, which is concurrent with the XRD study. After reduction of Cu and Ni metals by hydrazine in the Fig. 3(d)–(f), it can be seen that the well mono-dispersed Cu–Ni bimetallic nano particles are distributed on the functionalized graphene oxide sheets.
The SEM images of AAPTMS@GO (a), Cu–AAPTMS@GO (b), (1:1) Cu–Ni–AAPTMS@GO (c), (1:1) Cu(0)–Ni(0)–AAPTMS@GO (d), (1:2) Cu(0)–Ni(0)–AAPTMS@GO (e) and (2:1) Cu(0)–Ni(0)–AAPTMS@GO (f) are shown in Fig. 4. From these images, the broken smaller sheets observed are formed after functionalization due to the interaction between silane and functional group of graphene oxide surface in the presence of organic solvent. The surface morphology of the materials was not changed after reduction of metals with hydrazine.
Fig. 4 SEM image of (a) AAPTMS@GO (b) Cu–AAPTMS@GO (c) (1:1) Cu–Ni–AAPTMS@GO (d) (1:1) Cu(0)–Ni(0)–AAPTMS@GO (e) (1:2) Cu(0)–Ni(0)–AAPTMS@GO and (f) (2:1) Cu(0)–Ni(0)–AAPTMS@GO. |
EDX spectroscopy gives the evidence on the type of element existing in the specific area. The SEM-EDX mapping of (1:1) Cu(0)–Ni(0)–AAPTMS@GO sample is presented in the Fig. 5. From these images, the presence of silicon, carbon, nitrogen, oxygen, Cu and Ni in this material can be seen. Another most vital and valuable ability of the EDX technique is X-ray mapping of elements. The positions of particular elements emitting specific X-rays within a scrutiny field are indicated by unique colors. The maps of distribution of elements like Si, C, N, O, Cu and Ni are exposed individually and overlapped with the original image as shown in the Fig. 5. The elemental mapping survey reveals that the most active elements like Cu and Ni were uniformly distributed throughout the sample. ICP-OES was used to determine the percentage ratio of Cu and Ni in 5 wt% of (1:1) Cu(0)–Ni(0)–AAPTMS@GO catalyst and it was found to be Cu/Ni ratio 0.98 i.e., Cu is slightly lower loading than Ni. This may be due to Ni, more electronegative than Cu, which can more easily coordinate to the electron donating N atom of AAPTMS group present on the amine functionalized graphene oxide surface.
HRTEM was also used to further investigate the morphologies, diffraction pattern and lattice fringes of the materials. The different magnification of (1:1) Cu(0)–Ni(0)–AAPTMS@GO material with spherical nano particles can be seen in Fig. 6(a)–(e). From Fig. 6(g) showing the SAED pattern of the polycrystalline diffraction rings, (111) and (200) planes were indexed as the brighter inner diffraction ring and dimmer outer ring. The lattice fringe presented in Fig. 6(f) shows the single crystalline nature of the bimetallic alloy nano particles with characteristic d-spacings of 0.20 nm for (111) planes of both Ni and Cu. Therefore, it was confirmed that the solid solution constitutes both Cu and Ni.
Fig. 6 HRTEM image of different magnification of (a–e) (1:1) Cu(0)–Ni(0)–AAPTMS@GO (f) lattice fringes of (1:1) Cu(0)–Ni(0)–AAPTMS@GO (g) SAED pattern of (1:1) Cu(0)–Ni(0)–AAPTMS@GO. |
The TEM and HRTEM images of mono dispersed bimetallic nano particles with histogram of particle size distribution plot for the Cu–Ni nanoparticles are shown in the [Fig. 7(a) and (b)]. From this Fig. 7, the average diameter of particle size is calculated to be ∼4 nm with a narrow size variation.
Fig. 7 (a) TEM (scale bar = 100 nm) and (b) HRTEM (scale bar = 50 nm) image at high magnification with particle size distribution plot of the (1:1) Cu(0)–Ni(0)–AAPTMS@GO. |
Catalyst | Conv. (%) | Product selectivity (%) | |||
---|---|---|---|---|---|
HCAL | COL | HCOL | Others | ||
a Catalyst (150 mg), cinnamaldehyde (1.2 g), methanol (16 ml), time (1 h), and temp. (80 °C). | |||||
Cu–AAPTMS@GO | 39 | 26.5 | 30.0 | 42.4 | 1.1 |
Ni–AAPTMS@GO | 44 | 26.2 | 32.7 | 40.3 | 0.8 |
(1:1) Cu–Ni–AAPTMS@GO | 52 | 18 | 42.2 | 38.5 | 1.3 |
(1:1) Cu(0)–Ni(0)–AAPTMS@GO | 85 | 17.6 | 59.8 | 22.4 | 0.2 |
(1:2) Cu(0)–Ni(0)–AAPTMS@GO | 82 | 11.8 | 51.3 | 36.3 | 0.6 |
(2:1) Cu(0)–Ni(0)–AAPTMS@GO | 79 | 14.4 | 49.0 | 35.7 | 0.9 |
Temperature | Conv. (%) | Product selectivity (%) | |||
---|---|---|---|---|---|
HCAL | COL | HCOL | Others | ||
a Catalyst (150 mg), cinnamaldehyde (1.2 g), methanol (16 ml), time (1 h), and temp. (90–120 °C). | |||||
90 °C | 89 | 14.9 | 50.8 | 33.8 | 0.5 |
100 °C | 92 | 12.3 | 42 | 44.5 | 1.2 |
120 °C | 98 | 10.4 | 21.5 | 66.7 | 1.4 |
Table 3 presents the activity/selectivity of hydrogenation of unsaturated aldehyde by (1:1) Cu(0)–Ni(0)–AAPTMS@GO nano materials under same reaction conditions, but in different solvent media, such as water, methanol and isopropyl alcohol. The hydrogenation reaction with methanol as solvent gave better conversion and selectivity towards COL compared to other solvents. This could be due to higher dipole moment as well as higher solubility of hydrogen in methanol.
Solvent | Conv. (%) | Product selectivity (%) | |||
---|---|---|---|---|---|
HCAL | COL | HCOL | Others | ||
a Catalyst (150 mg), cinnamaldehyde (1.2 g), time (1 h), and temp. (80 °C). | |||||
Methanol | 85 | 17.6 | 59.8 | 22.4 | 0.2 |
Isopropyl alcohol | 62 | 22.6 | 51.1 | 25.6 | 0.7 |
Water | 57 | 45 | 21.8 | 32.8 | 0.4 |
In the current study the broader utility of Cu–Ni bimetallic graphene oxide nanocomposites as catalysts for hydrogenation of nitro phenol was investigated with NaBH4 as hydrogen source and water as solvent. The (1:1) Cu(0)–Ni(0)–AAPTMS@GO as catalyst gave highly impressive results with 100% conversion and selectivity towards p-amino phenol and reaction finished in 16 min at RT, while the 1:2 and 2:1 compositions recorded lower selectivity and conversions. These results prove superior to the literature reported results in terms of both conversion and selectivity efficiency and reaction conditions and time needed.
The hydrogen abstraction from BH4− and transferring to p-nitrophenolate anion occurred efficiently by the bimetallic alloy particles on the amino functionalised graphene oxide surface. The reduction of aromatic nitro compound was monitored by UV-Vis study. In UV-Vis, the peak at 400 nm indicates p-nitrophenolate anion and at 300 nm indicates the product of p-aminophenol with (1:1) Cu(0)–Ni(0)–AAPTMS@GO catalyst shown in ESI Fig. S3.† In Fig. S3(A),† shows the decrease in absorbance at 400 nm, due to the consumption of p-nitrophenolate anion intermediate and the increase of intensity at 300 nm due to the formation of product, p-aminophenol. The representative products were characterized by 1H NMR, 13C NMR and FTIR spectroscopies for conformational study in ESI Fig. S4(a–c).† (1:1) Cu–Ni–AAPTMS@GO catalyst showed very less activity due to the presence of different form of metallic phases, which was confirmed from the XRD results. However, the (1:1) Cu(0)–Ni(0)–AAPTMS@GO catalyst displayed the best catalytic activity towards p-amino phenol reduction, when compared to (1:2) Cu(0)–Ni(0)–AAPTMS@GO and (2:1) Cu(0)–Ni(0)–AAPTMS@GO. The high activity of (1:1) Cu(0)–Ni(0)–AAPTMS@GO was due to good dispersion of the (1:1) ratio of Cu–Ni bimetallic alloy nanoparticles on the functionalized graphene oxide sheets and the enhanced adsorption ability of graphene oxide for p-nitrophenol stems from the π–π stacking interactions. From Fig. S3(B) and (C),† it can be deduced that the reduction of nitro compound to amino compound over (1:1) Cu(0)–Ni(0)–AAPTMS@GO follow pseudo first-order kinetics for the chosen conditions.
Best features of ideal heterogeneous catalyst are high selectivity, high activity, long lifetime and cost effectiveness. The recyclability of the heterogeneous catalyst is vital parameter and it depends on its stability and the easy separability. The activity can change due to leaching of some metal particles into the reaction medium or may be the coke formation on the catalyst surface in the high temperature reactions. To test its robustness, the recovered catalyst was reused after regeneration followed by wash with water and calcination. No noticeable change up to 6th cycle was observed with activity remaining intact (Fig. 8). The catalyst did not leach out in this medium showing strong interaction between nanoparticles and amino group. The decrease in 7th circle could be due to some leaching Cu metal as compared to Ni. The binding capacity of Ni is higher than Cu, which can be more easily coordinated to the electron donating N atom of organic group present on the amine functionalized graphene oxide surface. The catalytic activity of hydrogenation of unsaturated aldehyde gives good conversion and selectivity and also the catalyst activity decreased (8%) in 5th cycle.
Fig. 8 The catalytic performance within seven cycles for the reduction of p-nitro phenol catalyzed by (1:1) Cu(0)–Ni(0)–AAPTMS@GO catalyst. |
The reduction of PNP to PAP performance of (1:1) Cu(0)–Ni(0)–AAPTMS@GO was evaluated and compared with the state of the art in the corresponding field in Table 4. The Pd/C and Pd/G catalysts46 the activity decreased in every cycle reaching 85% in the 5th cycle. With CuFe2O4 MNPs catalyst50 catalyst was stable up to 2nd cycles only. So, that our (1:1) Cu(0)–Ni(0)–AAPTMS@GO catalyst has better recyclability and reusability.
The XRD, FTIR, SEM, TEM, HRTEM analysis of sixth cycle of reused catalyst are shown in ESI Fig. S5.† In the XRD spectra of reused (1:1) Cu(0)–Ni(0)–AAPTMS@GO catalyst, the strong and active diffraction peak of nano particle at 2θ = 43.51° for (111) plane, disappeared in the 7th cycle, although it can be seen after recycling it for the 6th cycle catalyst [Fig. S5(a) and (b)†]. From FTIR also it can be seen that the stretching vibrations of Si–O–C peak vanished after 6th cycle in [Fig. S5 (c) and (d)†]. The SEM, TEM and HRTEM images [Fig. S5(e)–(g)†] of the 6th cycle reused catalyst show no obvious change in morphology of the nanoparticles i.e., well-dispersed nanoparticles as like the fresh sample. Agglomerated bimetallic Cu–Ni nano particles were observed in the SEM, TEM and HRTEM images [Fig. S5(h)–(j)†] of the (1:1) Cu(0)–Ni(0)–AAPTMS@GO catalyst reused after six times.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c6ra26443c |
This journal is © The Royal Society of Chemistry 2017 |