Manisha
Samanta
,
Satya N.
Guin
and
Kanishka
Biswas
*
New Chemistry Unit, Jawaharlal Nehru Centre for Advanced Scientific Research (JNCASR), Jakkur P.O., Bangalore 560064, India. E-mail: kanishka@jncasr.ac.in
First published on 1st November 2016
Layered materials with intrinsically low thermal conductivity are promising candidates for thermoelectric waste heat to electrical energy conversion. Recently bulk form BiCuSeO, a layered oxychalcogenide, has drawn attention for thermoelectric applications. However, synthesis of a two dimensional nanosheet of BiCuSeO and study of its thermoelectric properties have not been explored yet. Here, we present a facile surfactant free low temperature solvothermal synthesis of few layered ultrathin BiCuSeO nanosheets for the first time. Nanosheets of BiCuSeO exhibit a semiconducting band gap of 0.9 eV and p-type conduction. A dense hot pressed pellet of BiCuSeO nanosheets exhibits a superior power factor and lower lattice thermal conductivity compared to that of the bulk sample in the temperature range of 300–723 K.
Thermoelectric materials will play a pivotal role in future energy management by harvesting waste heat and converting it into electrical energy.9–11 Narrow band gap semiconducting inorganic solids are important materials for thermoelectric applications.9–11 Anisotropic materials with layered structures such as Bi2Te3, Sb2Te3 and Bi2Se3 have been enormously explored for thermoelectric applications.12–14 The anisotropic crystal structure and bonding result in substantial differences in the thermoelectric properties in different crystallographic directions. For example, SnSe, which is a layered narrow band gap semiconductor, exhibits ultralow thermal conductivity with a record high zT ∼ 2.6 along the crystallographic b axis.15–17
Layered quaternary metal oxychalcogenides, MCuXO (M = La, Ce, Nd, Pr, Bi, and In; X = Te, Se and S) have been found to be important materials for thermoelectrics, superconductivity and interesting electronic transport.18,19 The presence of covalent metal–chalcogen and ionic metal–oxygen units in the layered structure leads to unique structural chemistry and exciting properties. Preferential bonding of chalocogen and oxygen with one particular type of cation results in low dimensional structures in MCuXO, which leads to anisotropic electronic structures and properties.
BiCuSeO is an interesting material from the oxychalcogenide family and has recently gained attention for thermoelectric applications due to its low thermal conductivity.20 BiCuSeO is a multiband semiconductor and crystallizes in a ZrCuSiAs type layered structure with a tetragonal unit cell (space group P4/nmm).18–22 The crystal structure of BiCuSeO consists of insulating (Bi2O2)2+ and conductive (Cu2Se2)2− layers, which are stacked along the crystallographic c axis of the tetragonal cell (Fig. 1a). The (Bi2O2)2+ layers consist of distorted Bi4O tetrahedra (fluorite type structure), whereas (Cu2Se2)2− layers consist of distorted CuSe4 tetrahedra (anti-fluorite type structure).20,21 The phonon–phonon Umklapp processes originate from the scattering of phonons from the interface due to the layered structure, soft bonding and lattice anharmonicity, which result in low thermal conductivity in BiCuSeO.20 The thermoelectric properties of bulk BiCuSeO have been improved by a carrier engineering strategy using metal ion (e.g. Mg2+, Ca2+, Sr2+ and Ba2+) doping or introducing single and dual vacancies.21,23–27
Fig. 1 (a) Crystal structure of BiCuSeO demonstrating the layered structure.19 (b) Powder XRD patterns of as synthesized BiCuSeO nanosheets. (c) Optical absorption spectrum of as synthesized BiCuSeO nanosheets. |
A bottom-up wet chemical synthesis of inorganic solids in the form of 2D nanosheets/nanoplates is an effective strategy for tuning the thermoelectric properties of bulk layered materials.14,28,29 The ultrathin 2D form of layered materials can lead to the quantum confinement of carriers, which can cause an enhancement in the Seebeck coefficient. Effective phonon scattering from the interfaces of nanosheets may result in reduction of lattice thermal conductivity. The free standing single layered Bi2Se3 showed excellent thermoelectric properties compared to that of its bulk counterpart due to improved electronic transport and reduced thermal conductivity.28–31 Kinetically synthesized few layered nanosheets of intergrowth (MX)m(E2X3)n [where M = Pb; E = Bi; X = Te, Se] homologous compounds exhibit ultra-low thermal conductivity due to phonon scattering by the heterostructure interface.32,33 Recently, ultrathin nanosheets of SnSe and SnSe2 were synthesized by soft chemical synthesis, and showed a high power factor and low thermal conductivity.34,35 This motivated us to synthesize and study the thermoelectric properties of pristine BiCuSeO nanosheets.
Herein, we demonstrate a low temperature surfactant-free soft chemical synthesis of ultrathin (∼4–5 layers and 3–4 nm thick) BiCuSeO nanosheets for the first time. Large scale few layered BiCuSeO nanosheets were synthesized by the reaction of Bi(NO3)2·5H2O, Cu(NO3)2·3H2O and selenourea in the presence of KOH/NaOH under solvothermal conditions. Transmission electron microscopy (TEM) and atomic force microscopy (AFM) characterizations indicate the 2D nanosheet morphology of the sample. Room temperature optical absorption studies indicate that as-synthesized BiCuSeO nanosheets exhibit a band gap of ∼0.9 eV. A significantly low lattice thermal conductivity in the range of 0.55–0.4 W m−1 K−1 was measured in a hot pressed dense pellet of BiCuSeO nanosheets in the 300–700 K range, which is lower than that of the bulk BiCuSeO. Extensive phonon scattering from the interfaces of the layers, bond anharmonicity and nanoscale grain boundaries resulted in low thermal conductivity in BiCuSeO nanosheets. Undoped BiCuSeO nanosheets exhibit p-type conduction (carrier concentration ∼3.8 × 1018 cm−3) and a higher average power factor value than that of the bulk sample.
Thermal diffusivity, D, of the hot pressed sample with a 10 mm diameter and 2 mm thickness, was measured in the range of 300–723 K by using a laser flash diffusivity method in a Netzsch LFA-457 instrument. Temperature dependent heat capacity, Cp, was obtained using a standard sample (pyroceram) in LFA-457, and is slightly higher than the Dulong–Petit Cp value of BiCuSeO. The total thermal conductivity, κ, was calculated using the equation, κ = DCp·ρ, where ρ is the density of the sample. Electrical and thermal transport was measured in the same direction of hot pressing of the pellet.
Powder X-ray diffraction patterns (PXRD) of as synthesized BiCuSeO nanosheets could be indexed based on pure tetragonal BiCuSeO with the P4/nmm space group, with no other impurity phase being observed within the detection limits of PXRD (Fig. 1b). The time dependent study of the reaction indicates that 24 h is the optimum time required for the formation of pure BiCuSeO nanosheets (see the PXRD in Fig. S1, ESI‡). The optical absorption spectrum of BiCuSeO nanosheets shows a well-defined band gap of ∼0.9 eV (Fig. 1c), which is higher compared to that of bulk BiCuSeO (∼0.8 eV).20
In order to confirm the presence of Bi, Cu, Se and O elements and their oxidation states, XPS of the as synthesized BiCuSeO nanosheets was performed (Fig. 2). Two strong peaks at 157.8 eV and 163.2 eV with a peak splitting of 5.4 eV are due to spin–orbit coupling and can be best assigned to Bi 4f7/2 and Bi 4f5/2, respectively, which is in good agreement with the value of Bi(III). The doublet peaks at 932 eV and 952 eV correspond to Cu(I) 2p3/2 and 2p1/2, respectively. An additional small intensity peak located at 942.4 eV is due to the presence of a minor amount of Cu(II). The reason for the presence of the minor amount of Cu(II) is because of the surface oxidation of Cu(I) to the more stable Cu(II).36 The peak at 529.9 eV arises due to O 1s. Peaks due to Se 3d5/2 and 3d3/2 are observed at 53.1 eV and 58.1 eV, respectively. We have presented the total XPS survey scan spectra from the nanosheets in Fig. S2 in ESI.‡
FESEM, TEM and AFM microscopy studies have been performed to understand the nanoscale morphology and the structure of the synthesized BiCuSeO sample. The FESEM image reveals the 2D nanosheet morphology of the sample (Fig. 3a). EDAX analysis of the BiCuSeO sample indicates the presence of Bi, Cu, Se and O (inset of Fig. 3a). The weight percentage (wt%) and atomic percentage (at%) of all the elements present in BiCuSeO, calculated from EDAX analysis, are given in Table 1. The TEM micrograph further confirms the thin nanosheet morphology of the synthesised BiCuSeO (Fig. 3b and c). The lateral dimensions of the nanosheets range from 0.5 to 1 μm. The selected-area electron diffraction (SAED) pattern taken from a single sheet region depicts the single crystalline nature of the BiCuSeO nanosheets (inset of Fig. 3b). The inset of Fig. 3c shows a TEM image of the bent edges of BiCuSeO, which indicate the stacking of a few nanosheets, one over another. A high resolution TEM (HRTEM) image (Fig. 3d) of the BiCuSeO nanosheets shows a clear lattice spacing of 2.67 Å, which corresponds to the (111) interplanar distance of tetragonal BiCuSeO. The ultra-thin nature of the nanosheets was further confirmed by AFM (inset of Fig. 3d). The height profile obtained from a typical AFM micrograph indicates that a thickness of ∼3.4 nm corresponds to 4 layers of BiCuSeO with a lateral dimension of ∼1 μm. Fig. 3e shows the scanning transmission electron microscopy (STEM) image of the BiCuSeO nanosheets. Additionally, EDAX elemental mapping analysis on a selected area of the BiCuSeO nanosheets (Fig. 3e), which is presented in Fig. 3f, points out the homogeneous distribution of all the elements in the BiCuSeO nanosheets.
Element | wt% | at% |
---|---|---|
O | 3.83 | 22.35 |
Se | 21.82 | 25.81 |
Bi | 56.15 | 25.09 |
Cu | 18.2 | 26.75 |
Total | 100 | 100 |
The layered structure and low thermal conductivity of bulk BiCuSeO motivate us to measure the thermoelectric properties of the BiCuSeO nanosheets. In order to measure thermoelectric properties, pellets of the BiCuSeO nanosheets were made by hot pressing of the as synthesized nanosheet powder sample. Fig. 4 represents the temperature dependent thermoelectric properties of the BiCuSeO nanosheets. Temperature dependent electrical conductivity (σ) and the Seebeck coefficient (S) of the BiCuSeO nanosheets are shown in Fig. 4a. BiCuSeO nanosheets show superior σ values to the bulk sample throughout the measured temperature range (Fig. S3a‡).20 We have measured the p-type carrier in BiCuSeO to be ∼3.8 × 1018 cm−3 at room temperature, which is higher than that of the bulk BiCuSeO.20 We have estimated the carrier mobility (μ) in BiCuSeO nanosheets using the formula σ = nheμ, where e is the electronic charge. The estimated carrier mobility value is ∼25 cm2 V−1 s−1, which is slightly higher than that of the bulk pristine BiCuSeO (22 cm2 V−1 s−1).20 This is attributed to the increase in electrical conductivity in the nanosheet sample compared to that in the bulk.20 At room temperature, a σ value of ∼15 S cm−1 was measured for the BiCuSeO nanosheets, and remains almost the same with a value of ∼13 S cm−1 at 722 K. The positive value of S depicts p-type conduction in the BiCuSeO nanosheets. An S value of ∼223 μV K−1 is measured at room temperature which increases to ∼267 μV K−1 at 722 K (Fig. 4a). Although the S value for the nanosheets is lower than that of the bulk sample (due to an increase in the carrier concentration in the nanosheet sample), a large increase in the σ value resulted in a significant improvement of the average power factor (σS2) in the nanosheet sample compared to that in its bulk counterpart20 (see Fig. S3c, ESI‡).
Fig. 4 (a) Temperature dependent Seebeck coefficient (S) and electrical conductivity (σ) of the BiCuSeO nanosheets. Temperature dependent (b) total thermal conductivity (κ) and (c) lattice thermal conductivity (κlat) of the BiCuSeO nanosheets and bulk BiCuSeO.20 |
The total thermal conductivity (κ) of the BiCuSeO nanosheet sample in the range of 300–700 K along with κ of the previously reported bulk sample20 are presented in Fig. 4b, whereas thermal diffusivity (D) and Cp values of the BiCuSeO nanosheets are presented in Fig. S4, ESI.‡ We found that the BiCuSeO nanosheets exhibit a lower κ value throughout the measured temperature range compared to the bulk counterpart. A κ value of ∼0.56 W m−1 K−1 was measured at room temperature, which further decreased to 0.4 W m−1 K−1 at 675 K. The large decrease in temperature dependent κ compared to the bulk sample is attributed to the significant reduction of the lattice thermal conductivity (κlat) in BiCuSeO nanosheets (Fig. 4c). The κlat of BiCuSeO nanosheets is obtained by subtracting electrical thermal conductivity (κel) from the total thermal conductivity (κ), whereas κel is calculated using the Wiedemann–Franz law, κel = LσT, where L is the Lorenz number. L is derived by the fitting of the respective Seebeck coefficients, which estimate the reduced chemical potential assuming a single parabolic band, which is described elsewhere.37 Such a low κlat in the nanosheet sample originates from phonon scattering by the nano/meso-scale interfaces and grains in the hot pressed samples in addition to the interfaces of the layers and bond anharmonicity in the bulk BiCuSeO. A thermoelectric figure of merit (zT) value was estimated to be 0.2 at 722 K for the BiCuSeO nanosheet, which is higher than that of the bulk sample20 at that temperature.
Footnotes |
† We dedicate this paper to Prof. Mercouri G. Kanatzidis on his 60th birthday. |
‡ Electronic supplementary information (ESI) available. See DOI: 10.1039/C6QI00435K |
This journal is © the Partner Organisations 2017 |