Kui
Li‡
a,
Rong
Chen‡
a,
Shun-Li
Li
a,
Min
Han
a,
Shuai-Lei
Xie
a,
Jian-Chun
Bao
*a,
Zhi-Hui
Dai
a and
Ya-Qian
Lan
*ab
aJiangsu Key Laboratory of Biofunctional Materials, School of Chemistry and Materials Science, Nanjing Normal University, Nanjing 210023, P. R. China. E-mail: yqlan@njnu.edu.cn; baojianchun@njnu.edu.cn
bState Key Laboratory of Coordination Chemistry, School of Chemistry and Chemical Engineering, Nanjing University, Nanjing 210093, P. R. China
First published on 18th June 2015
We designed and successfully fabricated a ZnS/CdS 3D mesoporous heterostructure with a mediating Zn1−xCdxS interface that serves as a charge carrier transport channel for the first time. The H2-production rate and the stability of the heterostructure involving two sulfides were dramatically and simultaneously improved by the careful modification of the interface state via a simple post-annealing method. The sample prepared with the optimal parameters exhibited an excellent H2-production rate of 106.5 mmol h−1 g−1 under visible light, which was 152 and 966 times higher than CdS prepared using ethylenediamine and deionized water as the solvent, respectively. This excellent H2-production rate corresponded to the highest value among the CdS-based photocatalysts. Moreover, this heterostructure showed excellent photocatalytic stability over 60 h.
With respect to the limited photocatalytic stability of CdS, passivation layers and surface modifications have been adopted to protect it from oxidation.7a,11 Both of these methods can increase the lifetime of CdS but at the cost of deteriorating its H2-production rate, which is because of the inhibition of photocatalytic reactions by the passivation layer and the contamination of the heterostructure.5d,7a Indeed, the low H2-production activity and limited photocatalytic stability primarily result from the poor separation and transport efficiency of the charge carriers. If we can embed a modulating interface with a tunable lattice constant as well as band structure, and enhance the interface state between the semiconductor heterostructure to modify the charge separation and transport time and efficiency,12 the H2-evolution rate and photocatalytic stability could be effectively improved simultaneously.5d,13 Therefore, developing a semiconductor heterostructure with high photocatalytic activity and stability via carefully mediating the interface state is a subject of especial importance from both scientific and practical perspectives.
In view of the aforementioned ideas, a ZnS/CdS porous heterostructure with a mediating interfacial layer acting as a transport channel (Scheme 1a) has been prepared using cation exchange14 and post-annealing methods on the basis of the following points: (i) ZnS/CdS exhibits quasi-type II characteristics and efficient photocatalytic hydrogen evolution because of the acceptor states (Is, VZn) in ZnS.5d Moreover, the extensively investigated Zn1−xCdxS with tunable parameters and lower acceptor states than those in ZnS was selected as an interfacial layer;15 (ii) ZnS-ethylenediamine (ZnS(en)0.5) was adopted as a template for fabricating the porous ZnS/Zn1−xCdxS/CdS heterojunction,16 which is especially important for the water-splitting reaction because of its surface reaction characteristics;5a,c,17 (iii) a post-annealing process, which has been widely employed to improve the properties of oxides but has rarely been used in sulfide heterojunctions,16a,18 was adopted to improve the interface state and photocatalytic activity of the heterostructure sample whilst maintaining its heterojunction.
Herein, a ZnS/Zn1−xCdxS/CdS three-dimensional (3D) mesoporous heterostructure that exhibited a very high charge separation efficiency and H2-evolution rate was designed and successfully fabricated for the first time. The mediating Zn1−xCdxS interface, which possessed a tunable lattice constant and band structure, acted as the charge-carrier transport channel, which favored the improvement of the charge separation efficiency. Moreover, the H2-production rate and the stability of the heterostructure involving two sulfides were dramatically improved simultaneously via the careful modification of the interface state via a simple post-annealing method. The sample prepared with the optimal parameters exhibited an excellent H2-production rate of 106.5 mmol h−1 g−1 under visible light, which was considerably greater than that of the other previously reported CdS-based photocatalysts. Moreover, the heterostructure exhibited excellent photocatalytic stability over a period of 60 h. The well-modulated interface state is responsible for the substantially improved photocatalytic activity and stability.
Fig. 1 Scanning electron microscopy (SEM) and transmission electron microscope (TEM) images of (a), (c) ZC30 and (b), (d) ZC30-500, respectively. (e) Element mapping and (f) HRTEM image of ZC30. |
The X-ray diffraction (XRD) patterns of the samples with incremental Cd2+ content (Fig. S6a†) showed an increase of hexagonal and cubic phases of CdS resulting from the limited S source.20 However, the characteristic peak of ZnS did not disappear even in ZC75, further confirming that the interfacial solid solution inhibited complete cation exchange between ZnS and Cd2+. Moreover, the peak corresponding to Zn1−xCdxS slightly shifted to lower 2-theta values with increased Cd2+ content, and ZC30 exhibited a similar phase structure but with shifted peak positions compared to those of a ZnS and CdS mechanical mixture (Fig. S7†), thereby indicating the formation of a Zn1−xCdxS phase. As shown in Fig. S6b,† the post-annealing process dramatically improved the crystallinity of ZC30 without the formation of any extra phases. The peak corresponding to Zn1−xCdxS shifted to higher 2-theta values with increasing temperature, indicating that the content of Cd in Zn1−xCdxS decreased because of the reaction between ZnS and the interfacial layer at high temperatures. Fortunately, the ZnS/Zn1−xCdxS/CdS heterostructure was well maintained even at 650 °C because of the presence of the interface.
To further confirm the ZnS/Zn1−xCdxS/CdS heterostructure in the as-prepared samples, element mapping and high-resolution TEM (HRTEM) were used to investigate the element distribution and phase structure of ZC30 (Fig. 1e and f). S and Zn were distributed evenly throughout the entire skeleton of the nanoframe, whereas Cd was primarily distributed at the edge of the nanoframe; this result was further confirmed by the smaller ratio of Cd/Zn at the center of the nanoframe (Fig. S8†). As shown in Fig. 1f, the lattice fringe of the nanoregion centralized at the edge of the nanoframe could be indexed as CdS. The lattice constant of Zn1−xCdxS surrounding the CdS QDs increased as the distance to the CdS nanoregion increased, and the lattice fringe of ZnS was observed far from the CdS nanoregion. This composition gradient (corresponding to different band structures) and the in situ formation of a stably embedded interface could reduce heterostructure stress and defect concentration and hence improve the separation and transport efficiency of the charge carriers.9a,b Compared with the pristine ZC30, the ZC30-500 possessed a higher crystallinity with smaller CdS QDs. Fortunately, the CdS QDs could still be observed in ZC30-650 (Fig. S9†), indicating the important role of the interface in maintaining the ZnS/Zn1−xCdxS/CdS heterostructure.
The effects of the Cd2+ concentration and post-annealing process on the band structure of the ZnS/Zn1−xCdxS/CdS heterostructure were investigated using UV-visible diffuse reflection spectroscopy and are exhibited in Fig. 2a. The band edge of the heterostructure dramatically shifted to longer wavelengths in the sample with only 10 at% Cd2+. All of the samples exhibited similar Eg irrespective of the Cd2+ loading, which was in complete contrast to the Eg values of the Zn1−xCdxS solid solution.12a This result may have been attributed to the formation of CdS QDs resulting from the cation-exchange characteristics and the larger radius of Cd2+ (0.97 Å) relative to that of Zn2+ (0.74 Å).14a,21 Notably, the spectra of ZC10 and ZC30 showed two band edges, and the entire diffuse reflection spectra were divided into two regions, with regions I and II corresponding to absorption in the UV and visible regions, respectively. Egs in the visible and UV regions were calculated by the Kubelka–Munk (KM) method (Fig. S10†) and shown in the inset of Fig. 2a. The Eg in region I, which represented the Zn1−xCdxS solid solution, decreased with increasing Cd2+ concentration, which was consistent with the XRD results. The Egs in region II didn't change dramatically for the samples ranging from ZC10 to ZC75. ZC30-500 showed a slightly larger Eg of CdS (2.50 eV) than that in ZC30 (2.37 eV). This can be explained by the decreased size of the CdS QDs (Fig. S9a†) resulting from the reaction between a small amount of CdS and the interfacial layer.21 When further increasing the temperature to 650 °C, the drastic reaction of Zn1−xCdxS in ZC30-650 as confirmed by the XRD patterns (Fig. S6†) dramatically increased its band gap from 2.37 to 2.79 eV. The nitrogen and water vapor adsorption/desorption isotherms of the photocatalysts with different Cd concentrations are presented in Fig. 2b. ZC30 exhibited the highest water vapor and N2 adsorption volumes and a specific surface area (SBET) of 105 m2 g−1 (Fig. S11†), which was much larger than the other photocatalysts.2c,15,22 Fortunately, ZC30-500 exhibited a relatively high SBET of 43.6 m2 g−1, whereas ZC30-650 showed a very low SBET of 14.5 m2 g−1 (Fig. S12†).
The photocatalytic production of H2 by ZnS/CdxZn1−xS/CdS heterostructures with different Cd2+ content was compared under visible-light irradiation (λ ≥ 420 nm) (Fig. 3a).2c In contrast to the negligible visible-light hydrogen evolution activity in mesoporous ZnS, the H2-production rate drastically increased with the content of Cd2+ increasing from 2 to 30 at%. Further increasing of the amount of Cd led to a reduction in the H2-production activity. ZC30 exhibited the highest H2-evolution rate of 34.2 mmol h−1 g−1. The interface with a suitable band structure and lattice constant in ZC30 acted as a transport channel and increased the photocatalytic activity, whereas excess CdS may have acted as charge recombination centers and decreased the photocatalytic activity. Moreover, the maximum SBET and water vapor adsorption of ZC30 increased the number of reaction sites and the absorption capacity for photons and water molecules. The charge-carrier separation and transport efficiencies were further confirmed via electrochemical impedance spectroscopy (EIS) (Fig. S13†). The spectrum of ZC30 showed a smaller semicircle in the middle-frequency region when compared to ZC75 and CdS, indicating that it possessed the fastest interfacial electron transfer arising from the well-modulated interfacial layer. To qualitatively confirm the extremely important role of the interfacial layer on the H2-production activity, a sulfur source (Na2S) was added with the Cd2+ to inhibit the formation of the Zn1−xCdxS interface layer.5d,23 As shown in Fig. S14,† both the intensity of the CdS and ZnS phase got stronger with an increasing amount of the sulfur source. Correspondingly, the H2-production activity decreased dramatically because of the inhibited formation of Zn1−xCdxS.
The post-annealing method, which has been extensively employed to improve the properties of oxides but has rarely been applied to sulfide heterojunctions,16a,19 was adopted to investigate the effects of interfacial states on the photocatalytic H2-evolution activity of ZC30. As shown in Fig. 3b, the photocatalytic H2-evolution activity first increased and then decreased with increasing post-annealing temperatures. ZC30-500 exhibited the maximum H2-evolution rate of 106.5 mmol h−1 g−1, which was 152 and 966 times greater than those of CdS prepared using ethylenediamine and deionized water as the solvent, respectively (Fig. S15†). In contrast, at higher temperatures, more ZnS and CdS reacted with the Zn1−xCdxS interface which drastically increased the Eg and the thickness of the interfacial layer, and hence, decreased the photocatalytic activity. Moreover, the deteriorated microstructure and substantially decreased SBET was another explanation for the depressed H2-evolution activity in the samples prepared at higher temperatures. The photocatalytic H2-production activity of ZC30-500 was considerably higher than the other CdS-based photocatalysts (Table S1†),2a,5d,6b,7,16a,24 indicating the extremely important role of the mediated interfacial state in improving the charge-separation efficiency and photocatalytic activity. The result of the comparison between the photocatalytic stabilities of pristine ZC30 and ZC30-500 measured without renewing the sacrificial solution is presented in Fig. 3c. The pristine ZC30 exhibited a relatively good stability of 20 h because of the intimate heterojunction, efficient spatial charge separation and suitable band-structure matching.12a Interestingly, ZC30-500 exhibited a considerably higher H2-production rate and longer photocatalytic lifetime over 60 h in comparison to ZC30 because of its faster interfacial electron transfer as confirmed by its much smaller semicircle in the middle-frequency region (Fig. S13†). This result was attributed to the further improvement of interface state via the post-annealing process, thereby confirming the hypothesis that the improved interface state could simultaneously enhance photocatalytic activity and stability. Neither the microstructure nor the XRD patterns of ZC30-500 exhibited distinct variations after 60 h of photocatalytic reaction (Fig. S16†), further confirming its excellent photocatalytic stability.
The mechanism for the separation and transport of photon-generated charge carriers in the heterostructure is shown in Fig. 3d. Photo-generated holes from the valence band (VB) of CdS transferred to the defect states of the interfacial Zn1−xCdxS layer, which then transferred into the acceptor states of ZnS because of the lower acceptor states (VZn, Is) in Zn1−xCdxS than those in ZnS. The defect states related acceptor levels in ZnS and Zn1−xCdxS were confirmed by the photoluminescence (PL) spectra (Fig. S17†). All of the heterostructure samples and the solid solution samples prepared via a thermolysis method16a with different amounts of Cd2+ showed a similar peak position of the emission derived from different defect states (such as VZn) when compared to that in ZnS. These results indicated the constant energy level of the defect states in ZnS, heterostructure and solid solution samples with respect to their CB edge. These results were consistent with previous publications,5d,15 which reported that the peak position of the emission derived from the defect states (such as VZn) in Zn1−xCdxS is similar to that in ZnS and doesn't change with the variation of Egs derived from the different amounts of Cu2+ dopant. Consequently, the semiconductor with a lower CB edge possesses a lower defect (such as Is and VZn) related acceptor level. Meanwhile, the photo-excited electrons from the interfacial Zn1−xCdxS layer transferred to the CB of the CdS QDs, which was located on the outside of the heterostructure. As a result, the excellent photocatalytic activity and stability in the ZnS/Zn1−xCdxS/CdS heterostructure may have been a consequence of the combined effects of the following three factors: (i) the mediated Zn1−xCdxS layer exhibited tunable parameters and lower acceptor states (such as VZn) when compared to ZnS, which dramatically improved the matching between ZnS and CdS, and the separation efficiency of the photo-generated charge carriers; (ii) the post-annealing process drastically improved the interface state and the crystallinity of the ZnS/Zn1−xCdxS/CdS heterostructure and enhanced the charge separation and transport efficiency; and (iii) the large SBET of 105 m2 g−1 and interconnected 3D network in the mesoporous heterojunction drastically increased the number of the reaction sites.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c5sc01586c |
‡ These authors contributed equally. |
This journal is © The Royal Society of Chemistry 2015 |