Su Min Ahn‡
ab,
Hwan Yeop Jeong‡a,
Jung-Kyu Janga,
Jang Yong Leea,
Soonyong Soa,
Young Jun Kimb,
Young Taik Hong*a and
Tae-Ho Kim*a
aMembrane Research Center, Korea Research Institute of Chemical Technology (KRICT), 141 Gajeong-ro, Yuseong-gu, Daejeon 34114, Republic of Korea. E-mail: ythong@krict.re.kr; thkim@krict.re.kr
bSchool of Chemical Engineering, Sungkyunkwan University, Suwon, Kyunggi 440-746, Republic of Korea
First published on 16th July 2018
In order to increase the chemical stability of polybenzimidazole (PBI) membrane against the highly oxidizing environment of a vanadium redox flow battery (VRFB), PBI/Nafion hybrid membrane was developed by spray coating a Nafion ionomer onto one surface of the PBI membrane. The acid–base interaction between the sulfonic acid of the Nafion and the benzimidazole of the PBI created a stable interfacial adhesion between the Nafion layer and the PBI layer. The hybrid membrane showed an area resistance of 0.269 Ω cm2 and a very low vanadium permeability of 1.95 × 10−9 cm2 min−1. The Nafion layer protected the PBI from chemical degradation under accelerated oxidizing conditions of 1 M VO2+/5 M H2SO4, and this was subsequently examined in spectroscopic analysis. In the VRFB single cell performance test, the cell with the hybrid membrane showed better energy efficiency than the Nafion cell with 92.66% at 40 mA cm−2 and 78.1% at 100 mA cm−2 with no delamination observed between the Nafion layer and the PBI layer after the test was completed.
Generally, cation exchange membrane (CEM) and anion exchange membrane (AEM) are used for VRFB membranes. Nafion is commonly used as CEM for its high ionic conductivity and adequate chemical stability due to its hydrophobic backbone and sulfonic acid terminated side chains, although it poses a problem of high crossover rate of vanadium ions, leading to a decrease in coulombic efficiency (CE) and capacity fading, and also its high cost.9,10 Apart from Nafion, hydrocarbon-based sulfonated membranes with low VO2+ permeability and good proton conductivity for its rigid aromatic backbone and high ion exchange capacity are considered as CEMs for VRFBs.11,12 Despite all their advantages, there are still issues of low resistances to vanadium species (high susceptibility to VO2+ ion caused by the electron-rich aromatic group in the hydrocarbon-based membranes) and poor oxidation stability.13 AEM, which conducts anions such as SO42− has been developed for its low vanadium crossover rate compared to the conventional CEM, which can be explained by the Donnan exclusion effect, defined as an electrostatic repulsion between the positive functional groups in the AEM and the positive vanadium ions.14,15 Regardless of its low vanadium crossover rate, AEM also features a drawback of low chemical stability in highly oxidative environment.16 In order to enhance the disadvantages of these ion exchange membranes, membranes that utilize the size of pores to let only specific size of ions to cross by, also called the size exclusion effect, have been developed.17–19 Porous membranes without ion exchange group have shown improvements in stability, in spite of displaying a problem of vanadium crossover and complicated processing.20
There is an ongoing research for a different type of membrane that can be used in VRFB, using polybenzimidazole (PBI).21–23 Pristine PBI membrane is an electrically inert polymer displaying a very low conductivity of around 10−12 S cm−1.24 However, it possesses a partially negative nitrogen in the benzimidazole group, which can create an acid–base complex when doped with acid.25,26 Proton transport in acid-doped PBI is mediated by the acid molecules that are dissolved in the polymer matrix.27 The fixed positive charge prevents the vanadium ion crossover due to the Donnan exclusion effect, resulting in low permeability to vanadium species and high CE.28 PBI membrane also exhibits good thermal and chemical stability, high glass transition temperature, and high mechanical strength.29 Nevertheless, most studies on PBI electrolyte membrane for VRFB are focused in porous membranes because they do not show sufficient ion conductivity under standard sulfuric acid concentration (3–4 M) of vanadium electrolyte due to the low acid doping capability.19,30 By adding pores to the membrane, PBI has been widely used as porous membrane, increasing the acid doping level and improving the conductivity of acid doped PBI membrane.18
Enhanced acid uptake property of dense PBI membrane based on poly[2,2′-(2-benzimidazole-p-phenylene)-5,5′-bibenzimidazole] (BIpPBI), which has an additional benzimidazole side group, was studied previously in our team.31 The inclusion of additional benzimidazole side group increased the acid absorption capability and induced its amorphous structure with high free volume, contributing to better proton conductivity and lower resistance. Also, the nitrogen in the additional benzimidazole group augmented the Donnan exclusion effect, leading to lower permeability to vanadium ions. BIpPBI showed cell performance with high CEs (>99%) and energy efficiencies (EEs) (78–95%) under a wide range of current densities (20–100 mA cm−2). In the in situ chemical stability test of our previous study, where continuous charge and discharge cycles were carried out at 50 mA cm−2, BIpPBI had constant CE above 99% and a stable EE with a slight decreasing trend after 500 cycles, indicating excellent long-term stability in highly acidic and oxidizing environment. However, in the ex situ chemical stability test, in which the membranes were soaked into a solution of 0.1 M VO2+/5 M H2SO4, BIpPBI displayed less degradation compared to a conventional hydrocarbon membrane, although Nafion 115 had better chemical stability than both membranes, indicating that additional research for improving chemical stability of BIpPBI is needed.
Along with the study of different kinds of membranes composed of distinct polymer material as previously mentioned, study of hybrid membranes with at least two different polymer materials combined is steadily progressing.32–35 However, most of these hybrid membranes are generally orientated to improve the ion selectivity by integrating an additional layer.36–38 For instance, Austing et al. dipped polyethylenimine and Nafion ionomer alternatively to Nafion layer using a layer-by-layer (LbL) technique, increasing the ion selectivity towards proton and reducing vanadium cross over.38 Similarly, to improve ion selectivity, Li et al. deposited ultrathin Nafion film onto the poly(ether sulfone)-sulfonated poly(ether ether ketone) porous membranes.36 These hybrid membranes showed improvements in ion selectivity and reduction of vanadium crossover, but still have a limitation in increasing the chemical stability.
To increase the chemical stability of hydrocarbon membrane, our team collaborated in developing a hydrocarbon/Nafion bilayer membrane with a mechanical nano-fastener, where Nafion was applied onto a hydrocarbon membrane via 3D-interface interlocking (3D-IIL) method, a ball and socket joint structure that binds these chemically different structures with no additional interfacial resistance.39 The chemically dissimilar structures of hydrocarbon and perfluorinated Nafion membranes cause delamination when combined, hence, a strong interfacing adhesion needs to be achieved at the interface. The 3D-IIL fastened hydrocarbon/Nafion bilayer membrane showed excellent VRFB performance. The chemical stability was also superior compared to its pristine hydrocarbon membrane in the ex situ chemical stability test, indicating the protective layer of Nafion layer applied on top of the hydrocarbon membrane reduced oxidative degradation.
In this work, we developed a layered hybrid type membrane where Nafion ionomer was spray coated onto the BIpPBI membrane. The nitrogen in the benzimidazole group develops an acid–base complex with the Nafion ionomer, creating a strong interfacial adhesion preventing delamination. For this reason, a layered hybrid type membrane with excellent interfacial adhesion has been developed without any help of additional manufacturing process, such as 3D-IIL. The combined effect of Nafion's excellent chemical stability and BIpPBI's low permeability to vanadium ions magnified the advantages of both polymers. The layered hybrid type membrane of BIpPBI/Nafion showed low resistance and low permeability to vanadium ions. It also showed high EE and CE under different current densities in VRFB cell performance test.
In order to prepare hybrid type membrane, 10 wt% Nafion was dissolved in DMSO. The thickness and the uniformity of the membrane can be adjusted by the spray coating process and the hot-press process. Nafion solution was sprayed onto the BIpPBI membrane using a spray coater (LSC-300, Lithotech., Korea) operated with a nozzle air pressure of 250 KPa with a moving speed of 50 mm s−1. Polymer solution was injected at a rate of 0.5 mL min−1 using a syringe pump. The spraying nozzle was moved in the x-axis direction at a travelling distance of 5 mm. The sprayed membrane was then dried at 190 °C on a vacuum plate for 10 minutes, and a sprayed layer of 1–1.5 μm was obtained by one cycle of spraying. The number of spraying cycle was adjusted to obtain the desired thickness. After spraying, Nafion was evenly pressed using a hot-press with a temperature of 130 °C and pressure of 10 kgf cm−2 to decrease the fluctuation of the surface. The low Tg of Nafion, 110 °C, which causes compression bonding, enables a uniform coating layer.
The membranes were cut into 2 cm × 2 cm and were dried at 80 °C under vacuum for 2 days, and their thickness (Tundoped), length (Lundoped), and weight (Wunoped) at dried state were measured. The membranes were immersed in 4 M H2SO4 for 2 days at RT for acid doping. The wet acid-doped PBI membranes were wiped lightly with Kimwipes, and their thickness (Twet), length (Lwet), and weight (Wwet) were measured. To measure solely the weights of the acid uptake (Wdoped), the wet acid-doped membranes were dried at 80 °C under vacuum for 2 days to remove water. The acid doping level (ADL), acid uptake (WA), and water uptake (WW) were explored using the following equations,
ADL = [(Wdoped − Wundoped)/MH2SO4]/(Wundoped/MBIpPBI) | (1) |
WA (wt%) = [(Wdoped − Wundoped)/Wundoped] × 100 | (2) |
Ww (wt%) = [(Wwet − Wdoped)/Wundoped] × 100 | (3) |
(4-1) |
(4-2) |
Area resistance (AR) can be assessed using an impedance analyzer connected with a two-probe clip-cell. The Nafion 115 and BIpPBI membranes were immersed in 4 M H2SO4 at RT for 2 days beforehand. Using the following equation,
R = (R1 − R2) × S | (5) |
The ion conductivity can be obtained from the area resistance value above, using the following equation,
σ = L/RA | (6) |
(7) |
(8) |
(9) |
Hybrid type membranes were fabricated by spray coating Nafion ionomer on one surface of BIpPBI membranes varying the spraying thickness, shown in the schematic drawing in Fig. 1(a). From here on, the names of the hybrid membranes will be designated as BxNy, with x as the thickness of BIpPBI layer in μm and y as the thickness of Nafion layer in μm. The hybrid type membranes with coated Nafion ionomer can be verified in the SEM images of Fig. 1 and S1 (ESI†). To confirm the coating layer, hybrid membrane was analysed for F atoms in XPS analysis because Nafion contains F element in the molecular structure, while BIpPBI is absent of F element. Fig. S1(c) (ESI†) showed that the peaks of the F element appeared largely near the 686 eV on the Nafion coated surface. However, no peak was found on the uncoated side.
Fig. 1 (a) Schematic of the BIpPBI/Nafion hybrid membrane and its interface; cross sectional SEM image of (b) B20N5 and (c) B20N10. |
In an actual application of VRFB, membrane degradation occurs at the positive electrolyte side where the VO2+ ions induce chemical degradation.40 Therefore, the chemically stable Nafion layer would face the catholyte when assembled in a VRFB cell. Both B20N5 be and B20N10 membranes have Nafion ionomer at one side of the hybrid membrane, and the other side displaying only pristine BIpPBI membrane, as seen in Fig. S1 (ESI†). The cross-sectional image also confirms that the upper layers of B20N5 (Fig. 1(b)) and B20N10 (Fig. 1(c)) membranes with uniformly thick Nafion ionomer are coated onto the BIpPBI membrane. As we have expected, for hybrid-type membranes, stable interfacial adhesion without any noticeable defect was obtained successfully, as a result of strong acid–base complex between the benzimidazole group in BIpPBI and sulfonic acid group in coated Nafion ionomers.
As stated in eqn (2) and (3), the WW and the WA are calculated considering the whole membrane weight, including both the BIpPBI and the Nafion content. The pristine BIpPBI membrane showed WA of 65.5 wt%, demonstrating its excellent acid absorption ability. During the acid absorption process, water molecules were also absorbed into the BIpPBI membrane due to the osmosis and hydrogen bonding with sulfuric acid absorbed, resulting in high WW value of 46.2%. However, in 4 M H2SO4 bath, the Nafion membrane showed WA of 1.0 wt% and WW of 7.0 wt%, which are very low values because Nafion membrane does not create any acid–base interaction with sulfuric acid as BIpPBI does. Hybrid membranes, which combine both BIpPBI and Nafion, have intermediate values of 44.8 wt% WA and 20.9 wt% WW for B20N5 membrane and 38.7 wt% WA and 23.6 wt% WW for B20N10 membrane.
The ARs of pristine BIpPBI and hybrid membranes, B20N5 and B20N10, were measured at 4 M H2SO4, shown in Fig. 2. Nafion 115 had high AR of 0.25 Ω cm2 with a thickness of 125 μm, which was 4–5 times thicker than other membranes being evaluated. BIpPBI with a thickness of 25 μm displayed AR of 0.117 Ω cm2 and ion conductivity value of 0.0141 S cm−1 using eqn (6). Nafion 115 showed larger AR of 0.25 Ω cm,2 but relatively higher ion conductivity of 0.05 S cm−1. This is due to the Nafion 115's thickness of 125 μm, in which the thickness itself can generate large AR. However, when calculating the ion conductivity shown in eqn (6), the equation is divided by the thickness value, and thus the tendency for ion conductivity is reversed. For the hybrid B20N5 and B20N10 membranes, the ARs were 0.201 Ω cm2 and 0.269 Ω cm2, respectively, and the values of ion conductivity were 0.124 S cm−1 and 0.111 S cm−1, respectively. Using the AR per 1 μm for BIpPBI and Nafion membranes, theoretical resistance can be calculated, which were obtained as 0.151 Ω cm2 and 0.161 Ω cm2, respectively. This values are lower than the measured area resistance, indicating that an interfacial resistance has occurred between BIpPBI layer and Nafion layer. For this reason, the two hybrid membranes have higher ARs than BIpPBI and Nafion membranes and slightly lower ion conductivity values.
Fig. 4 (a) Schematic and (b) actual photo of the ex situ chemical stability testing apparatus; SEM images of (c) BIpPBI surface (d) cross section and (e) B20N5 surface (f) cross section. |
The chemical degradation of the BIpPBI and the hybrid membranes resulted from the strongly oxidizing VO2+ ions, which can be visibly seen in Fig. S2(d and e) (ESI†). When the BIpPBI membrane, weakened by the VO2+ ions, was teared off from the rubber gasket after the test, it created a perforation in the middle (Fig. S2(d) in ESI†). On the contrary, hybrid type membranes, B20N10 and B20N5, did not disintegrate during the tear off, and remained comparatively intact with only minor cracks (Fig. S2(e) in ESI†). SEM analysis was done after the ex situ chemical stability test on the surface and the cross section of the membranes, as seen in Fig. 4(c–f). After the accelerated test in 1 M VO2+/5 M H2SO4 solution, fractures were seen on the surface representing chemical degradation, especially for BIpPBI membrane (Fig. 4(c)). In the cross sectional image, more ruptures were found on the BIpPBI membrane (Fig. 4(d)) compared to the hybrid membrane (Fig. 4(f)). For hybrid membranes of B20N5 (Fig. 4(e and f)) and B20N10 (Fig. S2(f and g) in ESI†), Nafion layer was still attached to the BIpPBI layer when the membranes were pulled off from the rubber gasket. Even though the hybrid membranes were wrinkled, fractures were barely observable. The accelerated oxidizing environment affected the hybrid membranes. However, the Nafion protecting layer deterred the chemical degradation, and thus the membranes were kept all in one piece.
1H-NMR analysis was carried out to the membranes after the ex situ chemical stability test, and was compared to intact BIpPBI membrane, which had no chemical stability test done, presented in Fig. 5. BIpPBI membrane when exposed to 1 M VO2+/5 M H2SO4 solution showed pronounced change in shape at 7.6–8.2 ppm (d, f, g, h peaks), suggesting considerable chemical degradation has occurred on the phenylene structure in the benzimidazole rings in the highly oxidizing environment of 1 M VO2+/5 M H2SO4 solution. Also a new peak appeared around 9.0 ppm, additionally confirming chemical degradation of the BIpPBI membrane after the ex situ chemical stability test.
Fig. 5 1H-NMR spectra of (a) pristine BIpPBI; (b) B20N5, (c) B20N10, and (d) BIpPBI after ex situ chemical stability test. |
For the hybrid membranes, B20N5 and B20N10, the change of the peak shape was not observed at 7.6–8.2 ppm after the ex situ chemical stability test. Also, the intensities of the newly formed peaks of hybrid membranes at 9.00 ppm were smaller than the peak of chemically degraded BIpPBI membrane, signifying that hybrid membranes are less affected by the VO2+ ions in the accelerated ex situ chemical stability test, as expected.
The VE is affected by the ohmic polarization and varies inversely with the current density.41 Larger area resistance of membrane enlarges the internal resistance in the VRFB operation, leading to an unfavorable influence over the VE. Although Nafion 115 membrane had the highest AR of 0.25 Ω cm2 due to its thickness of 125 μm, when applied to VRFB single cell, all three singles cells showed similar VEs of 90–91%, 85–86%, and 81% in 40, 60, and 80 mA cm−2, correspondingly. At 40 mA cm−2, the single cell assembled with B20N10 had the highest VE of 91.39%. However, as the current density increased to 100 mA cm−2, the B20N10 cell displayed the lowest VE of 76.08%. At higher current density, the membrane resistance is more affected to the voltage efficiency.42 Therefore, B20N10 with the highest area resistance among the membranes, showed a larger drop of VE.
EE, a product of CE and VE, is the key parameter for the energy loss occurring during the charge–discharge process. With the combined effect of CE and VE, VRFB single cell fabricated with the hybrid membrane B20N10 showed highest EEs among the single cells with values of 92.66%, 87.55%, and 82.2% in 40, 60, and 80 mA cm−2, in the respective order. However, at a high current density of 100 mA cm−2, the order of EE value reversed for BIpPBI single cell (78.1%) and B20N10 single cell (76.84%) due to the high AR of B20N10. In spite of this overturn, the single cell assembled with B20N10 showed superior EE than the cell with Nafion 115 in all measured current densities. Cycling test was conducted to investigate long term stability of the membranes. Under 60 mA cm−2, the continuous charge and discharge test was conducted without replacement of electrolyte for 300 cycles. Fig. S4 in ESI† shows the cycling test efficiency and the discharge capacity of BIpPBI and B20N10. For CE, both membranes maintained 100% constantly due to low vanadium permeability. The BIpPBI kept stable EE of 90–87% for 300 cycles, and B20N10 maintained EE of 87–85%. Looking at the discharge capacity, BIpPBI showed decrease of 28.3% and Nafion coated B20N10 showed decrease of 19.8% in discharge capacity after 300 cycles. This confirms the less capacity loss of B20N10, implying due to the lower vanadium permeability, relatively less capacity retention occured. The CE and EE of Nafion 115 were stable. However, due to rapid capacity fade, the capacity retention decreased to less than 50% at 100 cycle.31 After the VRFB single cell performance test, the testing equipment was disintegrated to evaluate for any visible change in the membrane. No discernible delamination was observed after the test, implying that acid–base complex formed between the benzimidazole group of BIpPBI and the sulfonic acid group of Nafion functions as a successful latch between the two layers. Post analysis was carried out for SEM images with B20N10 and BIpPBI membranes to examine visually for any degradation in the surface or the cross section of the membrane after the VRFB single cell performance test, featured in Fig. S3 (ESI†). The membrane degradation is less distinctive than the ex situ chemical stability test that used 1 M VO2+/5 M H2SO4, revealing that in an actual condition of VRFB, membranes do not go through deterioration as much as they did in the accelerated ex situ chemical stability test. Moreover, the BIpPBI membrane (Fig. S3(d and e) in ESI†) showed more roughness and jaggedness on the surface and more cavities on the cross sectional images than the B20N5 membrane (Fig. S3(a–c) in ESI†), signifying that the Nafion protective coat on the surface of B20N5 deter membrane degradation against the oxidative environment of VRFB.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c8ra03921f |
‡ These authors contributed equally to this work. |
This journal is © The Royal Society of Chemistry 2018 |