Department of Materials, University of Manchester, Manchester M13 9PL, UK. E-mail: Xuqing.liu@manchester.ac.uk
First published on 10th January 2023
Smart wearable electronics are now of great significance in the fields of biomedical applications and environmental sensors. The development of new devices will be a continuing pivotal hotspot for human beings in future. However, contamination caused by large quantities of traditional electronic waste has already done serious damage to the reputation, especially the unignorable and irreversible environmental pollution caused by the leakage of heavy metal ions and plastic microparticles. To address the issues mentioned above, we design recyclable, flexible and stretchable homogeneous wearable sensors, which are hydrogen bonding crosslinked polyvinyl alcohol (PVA) conductive films, via applying ion-conductive 1-hexyl-3-methylimidazolium bromide ([HMIM]+Br−) ionic liquids, into a PVA polymer network by the freeze-thawing method. The application of [HMIM]+Br− (Br-IL) can guarantee stable conductivity with no effect on the recyclability of the whole device. What's more, Br-IL also endows the PVA film with tuneable properties, such as enhancing the flexibility and stretchability of films which is a challenge for polymer-based electronics. Not only that, Br-IL also creates a bi-continuous ion conductive phase structure in the polymer network, which could be called a “swimming lane effect”. Experiments successfully prove that the PVA/Br-IL ion-conductive films can be used for strain/temperature/humidity sensing applications with perfect recyclability and reusability.
Sustainability spotlightAccording to the UN's SDG Report 2022, about 80% of e-waste has been either burnt or disposed of in landfills. However, the majority of these electronic devices consist of plastics, heavy metals, and harmful substances, and such disposal methods will contaminate the atmosphere, soil, and water, especially since, according to reports, over 17 million metric tonnes of plastic have infiltrated the oceans. To ensure responsible consumption and production, we present a novel sensor based on theoretically unlimited recyclable polyvinyl alcohol and a green solution: an ionic liquid. This device composed completely of organic material could be recycled by simple dissolution and then reproduced as a sustainable device. |
In this context, for further developments in wearable devices without aggravating environmental contamination issues and high production costs, the concept of transient technology has been developed in recent years.15 Transient technology is an emergent technology that requires devices to “disappear” into a natural or common environment without traceable remains. This technology concept has already been successfully used to design biomedical applications and environmental sensors.16,17 In these devices, the components used based on transient technology can maintain their complete characteristics and operational functions with reliable performance under normal use conditions. After being recycled, these devices will have a controlled end to their life, for example by dismantling their structure and making them untraceable.
Based on this new concept, a recyclable polymer-based multifunctional sensor infiltrated with an ionic liquid (IL) is reported in this work. Polyvinyl alcohol is an often-tested synthetic polymer with well-known biocompatibility, solubility and easy processing characteristics.18–20 However, the pure PVA films could not always keep their strong mechanical properties and will be even worse if solid conductive materials were introduced, which would lead to phase separation of the solid particles under prolonged mechanical stress and ultimately to a reduction in performance. To overcome the stated problems, ionic liquids are added into the PVA polymer network which is proved to be a practical solution to prepare homogeneous biopolymer blends because of the non-volatility, recyclability, and ion-conductive properties of ionic liquids.21–23 Numerous experimental studies have shown that, when combined with different polymers, IL/polymer composites could provide a stable, versatile and often flexible sensing platform.24 Furthermore, based on a wide variety of IL functional characteristics, polymer/IL composites are allowed to be tuned for responses to multiple external environmental stimuli, such as heat and humidity.25
In the present work, this study reports on the development of a multi-response film sensor based on 1-hexyl-3-methylimidazolium bromide (Br-IL) and polyvinyl alcohol (PVA). Both materials show environmental safety and biodegradability, and so do the developed ion-conductive films. The PVA/Br-IL films' morphological, physico-chemical, thermal, mechanical and electrochemical properties were studied, together with their performance as a multi-sensing platform.
To explore the role of IL in the enhancement of PVA polymer networks, the morphology and microstructure of the as-obtained films were characterized using a scanning electron microscope (SEM), as shown in Fig. 2A(I)–(III). It is clearly observed that the pure PVA film shows a neat and smooth surface, while the PVA/Br-IL film consists of highly unidirectional entangled micro-fibrils, which indicates that the PVA film shows a higher crystallinity than the PVA/Br-IL film, as shown in Fig. 2B. All these fibrils at the macro level are manifestations of hydrogen-bonded PVA and [HMIM]+Br− chains at the micro level, and this indicates that [HMIM]+Br− will form a unidirectional network and entangle with the main polymer network to fabricate a homogeneous structure which is highly ordered with the benefit of zwitterions. Moreover, Fig. 2A(IV) and S1† show the size of a highly fine PVA fibre with [HMIM]+Br− modified down to hundreds of nanometres. It also can be found that the same aligned polymer chain is on the surface. This is because the fibre is made from polymer bulk and the fibre shape is the result of stretching when the orientation of PVA chains in the polymer is redirected. In addition, energy-dispersive X-ray spectroscopy (EDS) images of the PVA/Br-IL film, in Fig. 2A(V)–(IX), show that the Br element is well dispersed both on the surface and inside the film, which also means that most [HMIM]+Br− molecules form stable hydrogen bonds with water and PVA polymer backbones.
For polymer network characterization, as shown in Fig. 2C, the characteristic bands for [HMIM]+Br− were observed at 1166 cm−1 (C–N stretching) and 622–756 cm−1 (NH2 & N–H wagging). These characteristic peaks can also be observed in the PVA/Br-IL film. All these peaks show that [HMIM]+Br− has been sufficiently dispersed in the film. The broad peak between 3000 and 3600 cm−1 refers to the O–H bonds, which are provided by PVA and sufficiently bound water.26 Compared with pure PVA, there are two more small peaks observed from the curve of the PVA/Br-IL film, which indicates that [HMIM]+Br− provides more hydrogen-bonding points for the whole system to trap more bound water. Benefiting from the larger amount of bound water, it will be more effective in enhancing free-charged ions migrating between and across polymer chains under an electric field. In summary, the introduction of Br-IL can soften the polymer network and induce the direction of crystallization, which will improve the spatial orientation. Meanwhile, the better orientation of the polymer/Br-IL network will have a significant effect on the increase in conductivity. Moreover, the penetration of Br-IL into the PVA network can improve the anisotropic mechanical properties of the PVA film and anisotropic mechanical properties, such as flexibility. For convenience, unless otherwise specified, the ion-conductive PVA film with a content of 100 wt% [HMIM]+Br− was used for all tests.
![]() | ||
| Fig. 3 (A) Tensile stress–strain curves, (B) moisture regain, (C) opacity, and (D) photographs of PVA films with different concentrations of [HMIM]+Br−. | ||
The main reason for such a noticeable improvement between the pure PVA and modified films is that the function of the ionic liquid is similar to that of lubricating oil between polymer chains. It allows the polymer chains to have more displacement relative to adjacent chains, and as a result, the film will have a higher elongation ratio at the macro level. Besides, the hydrogen bonds between PVA chains are the main connection and will absorb energy during deformation. With the addition of ionic liquid, more hydrogen bonds can be formed not only between PVA chains but also between PVA and ionic liquids. Benefiting from the internal connection in the ionic liquid, which is an ionic bond, the double-bonded system containing hydrogen bonds and ionic bonds can have a much better buffer effect compared with the unitary hydrogen bond system.
What's more, it is worth noting that the resistance had a sharp drop at the instance when the finger started to bend instead of an increased resistance which is unlike what is observed for other common conductive materials, such as silver, copper and carbon, that is, the PVA/Br-IL film shows an unprecedented strain-induced ionic conductivity boost. Such a surprisingly opposite trend of strain-conductivity is similar to the work reported by Yao et al. It is concluded that IL will mainly solvate the soft spacers of the PVA region via selective cation adsorption, while rigid mesogens would force the anions to move only between them which contributes to ionic conductivity. Before stretching, the fibre network shows a nematic mesophase state with a slightly aligned polydomain. In this state, ions are dispersed and restricted in the network, which leads to a low ion transport behaviour. When the film is gradually stretched, an apparent nematic-to-smectic phase transition will happen between the polymer and ionic liquid and the ion-conducting performance will be boosted, thereby achieving ultra-fast ion transport performance which is similar to the role of “swimming lanes”, which is illustrated in Fig. 4B.
was found to decrease by nearly 8 times from 0 °C to room temperature. Meanwhile, it was also found that upon heating the sensor up to 85 °C, the resistance of the PVA/Br-IL temperature film sensor dropped slightly to under half that at room temperature. The same downward trend of resistance with temperature over the two periods of heating might be due to the dissociation of the ions. When freezing the film down to 0 °C, the crystallization zone in the interior of the polymer network will be more rigid and hinder the movement of ions. Also, anions and cations of the ionic liquid tend to form more coupling connections at lower temperature and this will hinder the accumulation of the ions at the interface between the film and electrodes. During the heating process, the stiff polymer network will be gradually softened and coupled ions will dissociate to become free anions and cations which can be driven under an applied electrical field. Moreover, the emergence of a substantial increase in resistance at the beginning of heating can be found in Fig. 4C. It might be concluded that the sudden temperature rise will dissociate a huge amount of free ions and this will result in a chaotic status that will also decrease the performance of directional movement of anions and cations.
Based on the unique thermal sensitivity behaviour of Br-IL, the film sensor could detect short-term temperature stimulations, even if this stimulus comes from the fingertip (Fig. 4D and S12†). Here, each time interval represents a complete contact cycle between the fingertip and the film sensor. A clear resistance change, in the range of 20–30%, could be found for each contact cycle. Also, like the strain sensor behaviour tests, the temperature-sensing behaviour was also tested in different environments (Fig. S9 and S10†). As illustrated in Fig. S9,† the same resistance change curves could be found when samples were at −2.5 °C and room temperature. However, completely opposite changes were observed in the
curves at 45 °C and that is due to the relatively low temperature of the fingertips which will contribute to the cooling of the contact area between the film and the fingertip, and that will further increase the resistance of the film. What's more, in Fig. S10,† the stable resistance change curves are the same as those in Fig. S9,† which indicates that such film sensors have a reliable thermal sensing performance in different environments.
The basic humidity-sensing response mechanism of the IL-based PVA sensor can be explained as follows. A series of models all consider the partition of water in polymer network uptake into two different ways which are commonly called bonded and unbound. Initially, when breathing out, a moisture-rich air flow filled the space between the medical mask and face. Once the IL-based PVA sensor has contact with the moisture, the chemical absorption of water will occur first. During this absorption process, the alcoholic hydroxyl group (Xn–OH) in the PVA molecular chain will change into the active state. The water molecule will establish hydrogen bonding with the hydrophilic sites on the PVA polymer. However, due to the introduction of the ionic liquid, a kind of strong amphoteric addition will result, with the PVA/Br-IL dual network already almost reaching its maximum dynamic balance of chemical absorption of water. Numerous hydrogen bonds have already formed and been stabilized among PVA, HMIM Br and water. Under this circumstance, the mechanism of moisture absorption will directly jump to the physical absorption and formation of unbound water. The physical absorption of water will continue by the corresponding water molecules attached to free hydroxyl groups in the deep narrow hollow space that still exists. Higher humidity levels give rise to a higher number of physically adsorbed layers formed in the shallow level of the whole system, which will still continuously lower the resistance of the film. And in the desorption process, along with the unbound water at a shallow level transported out of the PVA/Br-IL film, part of the unbound water at a deep level is still trapped and covered by the giant ionic liquid molecule which has undergone displacement. At this time, higher humidity levels mean more physically absorbed water layers formed and the removal of these layers is much slower. That may be the reason that, when breathing by mouth, the changing slope of desorption was rather lower than that of adsorption, which means the recovery time of the IL-based sensor is rather slower than the response time. Meanwhile for nose breathing, the recovery time of the sensor is almost the same as the response time. What's more, it is found that good moisture regain ability is like a “double-edged sword”. The PVA/Br-IL film is endowed with good humidity-sensing performance. However, the noticeable drift in the resistance–humidity curve can be attributed to the fact that during long-time cyclic breathing, part of the moisture was firmly captured by the film and could no longer vapourize from the system, which is gradually affecting the resistance during the test. Although there is a certain resistance deviation, the resistance curve is always similar, indicating that our hydrogel sensor has high durability in practical applications.
Mechanical tests also show that there is no obvious mechanical tensile property deterioration after several cycles, as shown in Fig. 5A. The good sensing and mechanical retainability of the PVA/Br-IL films ensure the recycling usage ability. What's more, benefiting from all water-soluble chemicals, as the number of cycles increases, the attrition rate still remains within a manageable range (Fig. 5B). Therefore, compared with conventional sensors based on non-degradable materials like metals, silicon and other traditional solid polymers, the PVA/Br-IL film sensor has the advantage of reusability and recyclability. In addition, different from previously reported recyclable sensors which require not only extreme conditions like strong acid or alkali conditions but also long-time operation for improving the recycling ratio, the PVA/Br-IL based sensor can be fully dissolved in hot water within several minutes, which is convenient, rapid and energy saving for the recycling process.
![]() | ||
| Fig. 5 (A) Tensile stress–strain curves of the primary PVA/Br-IL film and recycled film, and (B) recycling attrition rate of the PVA/Br-IL film. | ||
000–186
000), 1-methylimidazole (≥99%) and 1-bromohexane (98%) were purchased from Alfa Aesar. Silver nanowires (diam. × L 120–150 nm × 20–50 μm, 0.5% (isopropyl alcohol suspension)) were purchased from Sigma-Aldrich. Poly(vinyl alcohol) and silver nanowires were used without further purification, and deionized water was used for all experiments.
The morphological structure of the PVA and PVA/Br-IL films/fibres was observed by scanning electron microscopy (SEM), using a Zeiss Ultra 55 FEG-SEM operated at a 1.5 kV/3 kV acceleration voltage, which depends on different samples. Energy-dispersive X-ray spectroscopy (EDX) was also performed at a 15.0 kV acceleration voltage. To prepare the sample, cut PVA and PVA/Br-IL films were fixed on a metal stub with carbon tape and were then coated with 5 nm of gold/palladium alloy using a Quorum Au/Pd coater.
High-resolution powder X-ray diffraction (XRD) was applied to reveal the crystalline and amorphous structures of the PVA and PVA/Br-IL films/fibres and the measurements were conducted at room temperature on a PANalytical X'Pert Pro (model XRD5) versatile machine.
Thermogravimetric analysis (TGA) was carried out from 30 to 750 °C under a nitrogen atmosphere (90.0 mL min−1) using a TGA Q500 thermogravimetric analyzer. Samples (5–10 mg) were analyzed in a platinum pan with 10 °C min−1 being the heating rate.
An Instron 5564 tensile test machine equipped with a 100 N load cell was used to test all the mechanical properties in the conditional room. The stress/strain measurements were carried out with film samples which were cut into a dumbbell shape at an elongation speed of 30 mm cm−1. The tensile strain was calculated by dividing the distance between clamps by the original length of the samples, and the tensile stress was measured by dividing the applied force by the cross-sectional area. Young's modulus was estimated from the initial slope of the stress/strain curve.
An Elrepho 450X spectrophotometer was used to test the optical properties in the conditional room. The colour, brightness, opacity, diffuse reflectance factors, yellowness, and whiteness of the prepared samples were tested at 10 nm intervals in the 400–700 nm visible spectrum.
An IviumStat.h electrochemical workstation from Ivium Technologies B.V. was used to test the electrochemical properties of the prepared samples. An MFIA 500 kHz impedance analyzer from Zurich Instruments along with the IviumStat.h was used to evaluate the multi-sensing performance of the PVA/Br-IL film. Samples were cut 1 cm wide by 5 cm in length. Copper tape and wires were used to connect samples to the instruments. All tests were carried out in the conditioning room unless otherwise specified. Normal surgical masks were used to simulate the breath under a medical face mask.
The films prepared for moisture regain measurement were dried to constant weight at 60 °C in a vacuum oven. Films before and after drying were accurately weighed and recorded as W0 and W1. All the tests were repeated more than three times and the moisture regain value was calculated using:
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d2su00040g |