Melina
Arcidiácono
a,
Juan A.
Allegretto
ab,
Omar
Azzaroni
a,
Paula C.
Angelomé
*c and
Matías
Rafti
*a
aInstituto de Investigaciones Fisicoquímicas Teóricas y Aplicadas (INIFTA), Departamento de Química, Facultad de Ciencias Exactas, Universidad Nacional de La Plata, CONICET, CC 16 Suc. 4, B1904DPI, La Plata, Argentina. E-mail: mrafti@quimica.unlp.edu.ar
bLaboratory for Life Sciences and Technology (LiST), Department of Medicine, Faculty of Medicine and Dentistry, Danube Private University, 3500 Krems, Austria
cGerencia Química & INN, Centro Atómico Constituyentes, Comisión Nacional de Energía Atómica, CONICET, Av. General Paz 1499, 1650, San Martín, Buenos Aires, Argentina. E-mail: angelome@cnea.gov.ar
First published on 13th January 2024
Sub-micrometre thin alternate bilayers of materials with appropriate refractive index contrast are widely used for the assembly of sensors based on the stimuli-responsiveness of such 1D photonic crystals (PC). A new degree of complexity was recently enabled by the availability of highly ordered multiporous materials. Specifically, we studied the integration of two kinds of materials with different refractive indexes: Si- and Ti-based highly ordered mesoporous oxides with defined pore sizes, and both Zr- and Zn-based Metal Organic Frameworks (UiO-66 and ZIF-8 MOFs), featuring microporosity and chemically tunable affinity. Synthesis conditions must guarantee the preservation of structural and chemical integrity when both building blocks are assembled into bilayers. Thus, we studied the influence of usually employed synthetic procedures for the selected individual materials on the available porosity, crystalline structure, and morphology of the obtained bilayers, and propose suitable paths for the integration of multilayers capable of acting as 1D-PCs with both meso- and microporosity.
An increasingly popular alternative employed to circumvent the above discussed shortcomings is to enrich structural and chemical tunability of 1D-PCs through the inclusion of porous materials belonging to the well-established family known as Metal Organic Frameworks (MOFs).20 MOFs are materials based on the non-covalent combination of metallic ions and multidentate organic linkers into 3D ordered structures that feature permanent porosity. Since the appearance of pioneering studies reporting their interesting adsorption properties,21,22 MOFs have raised an ever-increasing interest due to a myriad of possible applications in diverse fields such as separation, catalysis, sensing, energy, or drug delivery, just to mention some of the most relevant examples.23–29,77 The potential of MOFs as building blocks for optical sensors and PCs has not gone unnoticed.30 Following the seminal contribution by Hupp et al. of a Fabry-Pèrot MOF-based vapour sensor,31 research efforts along this line have increased substantially; interesting reports include direct nanoparticle self-assembly for RI contrast,32–35 and filling or imprinting strategies for the nanofabrication of patterned surfaces acting as 2D-PCs.36–38 Due to the nature of building blocks, when employing MOFs for the assembly of 1D-PCs, additional materials must be included in order to guarantee the necessary RI periodic variation. Such RI contrast has been achieved by combining bilayers of MOFs and dense oxide nanoparticles or films (typically SiO2 or TiO2).39–43 However, the combination of MOFs with highly ordered surfactant-templated MTFs such as those obtained via sol–gel chemistry bears the potential for constituting a new generation of 1D-PCs but remains virtually unexplored. For such an end, if multiple bilayers are to be integrated into photonic nanoarchitectures, the (unfortunately not straightforward) compatibility requirement between synthetic routes for both materials must be met. This is an essential step towards the rational organization of nanostructures into functional materials, i.e.: “nanoarchitectonics”.44,45 Template-extraction and calcination steps required for MTFs might irreversibly affect the MOF phase; and conversely, MOF synthesis conditions typically involve organic solvents and/or strong acid modulators that might cause disruption of the MTF structure via template extraction or induce further changes through dehydration of metal oxide/oxyhydroxide moieties. Preparation methods must also ensure the necessary stratification and controlled thickness of alternate stacks, avoiding, for example, interpenetration generated by cross-diffusion of precursors. Aiming to identify strategies yielding bilayers and employing archetypal materials of each class, we explored the synthesis of bilayers composed of TiO2- and SiO2-based MTFs with different pore sizes13 and combined them with two selected MOFs, namely, Zr-benzene dicarboxylic acid-based UiO-6646 and Zn-methylimidazolate-based ZIF-8.47 We were able to identify critical steps and adapt typical synthetic procedures employed for the selected individual building blocks to preserve structural integrity. Evaluation was carried out in terms of key parameters such as available porosity, structure, and crystallinity. Finally, bilayers were assembled using building blocks in different orders, adapted protocols for template extraction and calcination procedures for mesoporous oxides, and synthesis/purification methods for MOFs to identify appropriate routes that would be feasible for the fabrication of multiporous 1D-PCs.
A defined volume (ranging from 75 to 100 microliters, depending on the substrate size) was deposited by spin coating at 4000 rpm over silicon or glass substrates previously cleaned with acetone and dried with air. Immediately after deposition, the films were subjected to a stabilisation process consisting of the following consecutive steps: 30 minutes in a 50% relative humidity chamber (obtained using a saturated solution of Ca(NO3)2), 30 minutes in an oven at 60 °C, 30 minutes in an oven at 130 °C and finally 30 minutes in an oven at 200 °C. The elimination of the template was performed either by extraction for 48 h with ethanol (films hereafter referred to as X – 200 + EE) or calcination at 350 °C for 2 hours, using a 1 °C min−1 ramp (hereafter referred to as X – 350).
APTES grafting of TB films was performed using a vapour-phase approach. The films were arranged in a 10 mm Petri dish box and an aluminium container filled with 500 microliters of APTES was placed alongside. Then, the box was covered and let to react for 20 minutes. After reaction, the films were placed for 15 minutes in an oven at 60 °C for thermal annealing.52
Ellipsometry experiments were carried out using a Woolan Alpha-SE Spectroscopic Ellipsometer equipped with a CCD detector and rotatory compensator (spectral range: 380–900 nm), at 70° incidence angle.
X-Ray Reflectometry (XRR) and X-Ray Diffraction (XRD) measurements were performed using a PanAlytical Empyrean diffractometer using a dedicated thin film optic, with an incident beam of Cu Kα radiation (1.54 Å). For XRR, a 1/32° divergence slit and a 0.18 mm receiving slit were mounted. Measurements were performed in a chamber that allows the atmosphere control by either introducing silica gel (dry atmosphere) or hot water (vapour saturated atmosphere). Details about these measurements and the data processing can be found elsewhere.62–64 The same configuration, but with a 1/16° divergence slit, was used to measure in the 2θ region corresponding to the mesoporous order peak (2–5° 2θ). Grazing incidence (GI-XRD) measurements, on the other hand, were performed with incidence fixed at 1° and scanning the 4–10° 2θ range, using a 1/2° divergence slit and none receiving slit.
Scanning Electron Microscopy (SEM) measurements were performed using Zeiss Crossbeam 340 Gemini equipment. Samples were cut into small pieces and fixed to an aluminium stub using conductive carbon tape. Transmission Electron Microscopy (TEM) measurements were performed using a Philips CM 200 microscope operated at 160 kV. Samples were scratched from the substrate using a scalpel and the obtained powder was deposited onto a FORMVAR and carbon-coated Cu grid. Dynamic Light Scattering (DLS) measurements were carried out using a ZetaSizer Nano-ZS90 (Malvern Instruments Ltd.). Surface area determination was carried out with an ASAP 2020 HD88 surface area and porosity analyzer (Micromeritics).
Fig. 1 Schematic representation for the obtention of LPE and SC MOF films, together with MTFs, and the combinations explored. |
It has been previously shown that continuous ZIF-8 films can be obtained using properly modified substrates, by introducing primer layers featuring chemical moieties capable of enhancing heterogeneous nucleation.48 The selection of such primer as well as the grafting strategy will determine the surface density of nucleation points in the substrate and thus will affect the growth extent and final morphology of the film.65 When using APTES as the primer, the films feature relatively high constructional porosity (CP, i.e., empty spaces in the meso-scale range across the film arising from defects and gaps generated in the spots where the growth fronts coalesce) in addition to the inherent ZIF-8 MOF microporosity. CP has been shown to play a significant role in adsorption and transport properties of films.29,66 This makes determination of the total accessible porosity far from trivial, since it includes both porous domains: intrinsic microporosity and meso-scale CP, which can even introduce domains with different specific affinities.
As can be seen in Fig. 2a(i), the (110) diffraction peak from ZIF-8 is present at 2θ = 7.35°, meaning that the native microporous structure of the MOF is present. It is worth noting that due to its low thickness (153 nm value was determined with ellipsometry for 5x-ZIF-8 LPE, see Section S2, ESI†) diffraction peaks corresponding to the 1x-ZIF-8 LPE film are not visible, and thus there is a necessity of performing XRD using thicker 5x-ZIF-8 LPE films. Nevertheless, 1x-ZIF-8 LPE could be used to measure XRR patterns. The critical angle measured by XRR is defined as the 2θ value for which the intensity of reflected X-rays is reduced to half of the maximum and can be directly related to the electronic density of the film.67 Thus, by comparing values corresponding to dry and water-saturated atmospheres, it was possible to analyse water-accessibility of the material. For ZIF-8, given the intrinsic hydrophobic nature of microporosity, the variation observed accounts for the accessible and more hydrophilic CP (see discussion below). In the same way, XRD and XRR experiments were conducted on ZIF-8 SC films as shown in Fig. 2b, which also showed the characteristic (110) diffraction peak and critical angle, denoting the presence of the synthesised material. For the case of the UiO-66 LPE film (Fig. 2c), XRD revealed a preferential orientation of the (111) plane, in line with previously reported results.68 Furthermore, the critical angle observed for the UiO-66 LPE film has a shift upon water adsorption, in line with the increased hydrophilic character of the micropores present compared with ZIF-8.69 AFM images show a uniform MOF coverage and the morphology and size of particles (or grain boundaries arising from colliding nucleation fronts during LPE) which integrate the films. Finally, Fig. 2d shows the diffraction pattern and XRR curves for the TB 200+EE film. In this case, milder extraction protocols implemented yielded a smooth and homogeneous film, as confirmed by the presence of Kiessig fringes in the XRR pattern. The presence of a well-ordered array of mesopores is confirmed by the appearance of a diffraction peak at 3.5° 2θ in the GI-XRD pattern of the sample (Fig. 2d(i)), corresponding to a periodic arrangement of mesopores with an interplanar distance of 2.5 nm in the direction perpendicular to the substrate. The mesopores and their long-range organisation are also visible on the film surface, as denoted by the SEM image presented in Fig. 2d(iii) and S3, ESI.† XRR curves evidence a shift due to capillary condensation when using dry and vapor-saturated conditions thus confirming the accessibility of the mesopores. Similar results, regarding the MTF accessibility, were obtained for SB 200+EE, TF 200+EE and TF 350 systems, in accordance with previous reports (Fig. S4 and S5, ESI†).49–51
Through spectroscopic ellipsometry (SE), thicknesses and refractive indexes (corresponding to 632 nm wavelength) were determined for the films employing ad hoc optical models. With this information, it was possible to apply effective medium approximation to obtain total porosities.
As presented in Table 1, all single layers present thicknesses between 70 and 250 nm, but with very different refractive indexes and porosities. It is worth noting that porosity values determined after applying Bruggemann approximation on ellipsometric measurements and those determined by XRR differ from each other. In the case of the 5x-ZIF-8 LPE layer, the difference in the values resides on XRR probing only the water-accessible porosity of the layer, while the 64% porosity found by Bruggemann's approximation arises from considering both contributions, the intrinsic microporosity of ZIF-8 (hydrophobic) and the more hydrophilic constructional porosity.54 In the case of the ZIF-8 SC layer, the high porosity value obtained by ellipsometric measurements points towards a less compact structure being formed; however, the interparticle space upon assembly seems to be too large to allow the capillary condensation. In fact, after exposing the film to a high RH medium during a long time, no changes in the ellipsometric signal were observed (Section S6, ESI†). In the case of UiO-66, given the more hydrophilic character of its porosity, it is likely that under 15% relative humidity conditions the porous material had adsorbed more water than the other MOF, thus hindering a larger change in electronic density upon increasing to 94% RH, which would justify the difference with the ellipsometric value found for the porosity. Also, it might be possible that not all the porosity was accessible due to occlusion of solvent or remaining reactants, despite the thorough washing and activation procedures followed. Finally, for the TB 200-EE sample, differences between the values obtained by the two techniques have been observed before for similar systems.70 Such differences may be due to the hydration equilibrium achieved in each kind of measurement and the fact that template may remain inside the films in different amounts, depending on the extraction process and subsequent cleaning of each sample. Nevertheless, the pore accessibility of TB 200-EE is high enough to ensure its use as a component of optical devices. TB 350, TF and SB layers were characterized by XRR, and the obtained thicknesses and porosities are in accordance with previously reported results.
System | Thickness(nm) | n(λ=632nm) | Porosity determined by ellipsometry | Porosity determined by XRR |
---|---|---|---|---|
5x-ZIF-8 LPE | 153 | 1.324 | 64% | 28% |
ZIF-8 SC | 203 | 1.171 | 80% | — |
UiO-66 LPE | 250 | 1.620 | 46% | 24% |
TB 200+EE | 135 | 1.643 | 29% | 39% |
TB 350 | 74 | — | — | 35% |
TF | 176 | — | — | 38% |
SB | 183 | — | — | 48% |
Altogether, results summarised in Table 1 show that the single layers can be grown homogeneously, rendering films with very different refractive indexes and porosities, which makes their combination an attractive path towards 1D-PCs development.
As can be seen from XRR experiments presented in Fig. 3a, spin-coating allowed the assembly of ZIF-8 nanoparticles on top of the TB 200+EE film (TB 200+EE/ZIF-8 SC). The XRR curve shows the appearance of an additional critical angle below 2θ = 0.2°, corresponding to ZIF-8, and the conservation of both the critical angle and the Kiessig fringes from the MTF. The latter indicates that the homogeneity of the TB 200+EE film is preserved (see Fig. S7, ESI† for the full-range XRR curves). However, the critical angle attributed to ZIF-8 is much lower than the one of the single layer presented above, indicating a lower electronic density, which points towards a lower surface coverage. This might be due to the different wettability of the TB 200+EE film compared with the APTES-modified silicon substrates, thus rendering a low-density assembly of nanoparticles. GI-XRD experiments also show no diffraction peak from ZIF-8, thus supporting the formation of a thin deposit of particles. Dry and water-saturated XRR experiments reveal that the TB 200+EE film is still accessible to water (22% accessible porosity), although some reduction of this parameter is observed, probably due to the presence of the ZIF-8 crystals on the surface, that might hinder water diffusion. Moreover, the upper ZIF-8 SC layer does not take up much water, also in line with ellipsometry results (see Fig. S6, ESI†).
Fig. 3 XRR experiments for dry and vapour-saturated atmospheres for samples: (a) TB 200+EE/ZIF-8 SC, (b) ZIF-8 SC/TB 200+EE, (c) TB 200+EE/5x-ZIF-8 and (d) 1x-ZIF-8/TB 200+EE. |
For the inverse configuration (ZIF-8 SC/TB 200+EE bilayer), the ZIF-8 SC layer was used as the starting point for the preparation of the MTF. Fig. 3b, shows the XRR pattern in which Kiessig fringes associated with the MTF layer (which also shows the expected diffraction peak attributed to the mesopore ordering, see Section S6, ESI†) are observed. Moreover, the MTF remains accessible to water (26% accessible porosity). In this configuration, in which the upper layer (TB 200+EE) is the one with the higher electronic density, the critical angle of the bottom layer (ZIF-8 SC) is not expected to be seen. However, there is no evidence of ZIF-8 being still present in the substrate, since no diffraction peak ascribable to it was detected, although it was clearly visible in the original single layer before MTF deposition (see Fig. 2b–i). This result suggests that adherence of the nanoparticles constituting the ZIF-8 SC single layer is compromised by the MTF synthesis procedure, regardless of the adaptations introduced for its compatibility with ZIF-8 MOF.
As an alternative, ZIF-8 layers grown by the LPE method were also explored. When starting from the TB 200+EE film, the oxide must be modified with a primer, to allow the anchoring of MOF precursors which later promote film growth. For this purpose, amino moieties (anchored using APTES) were employed as nucleation points for ZIF-8, thus generating the TB 200+EE/ZIF-8 LPE bilayer. It was observed, however, that more than one growth cycle was needed for the presence of ZIF-8 to be detectable. By taking advantage of the progressive growth achievable via LPE, five growth cycles were conducted, thus generating the TB 200+EE/5x-ZIF-8 LPE bilayer. Crystallinity of the system was explored and quite interestingly a wide diffraction peak around 6.75° 2θ was observed instead of the expected peak at 7.35° 2θ. Such a result points towards the formation of a crystalline phase other than ZIF-8 due to the interactions between MOF precursors and the mesoporous film. This could also explain why when performing low- and high-moisture XRR experiments (see Fig. 3c) the porosity of the TB 200+EE layer was no longer accessible to water, since no displacement of the critical angle is observed for higher humidity. Altogether, this suggests that mesopores are being blocked by subproducts generated while attempting the synthesis of ZIF-8, blocking the access to MTF porosity. For the inverse configuration (1x-ZIF-8/TB 200+EE), again no diffraction peak for the ZIF-8 phase was observed. We hypothesise that this could be due to its low thickness, but again no structures related to ZIF-8 MOF were detected with electronic microscopy (neither SEM nor TEM). Nonetheless, a 130 nm thickness MTF film was successfully grown on the modified substrate. Such a MTF presents accessible mesopores (31% porosity, obtained from XRR shown in Fig. 3d) and an ordered pore array that gives rise to a diffraction peak at 3.25° 2θ, corresponding to an interplanar distance of 2.7 nm (see the XRD pattern in Fig. S8, ESI†).
Altogether, the formation process of the MTF seems incompatible with the production of ZIF-8/MTF bilayers and further steps are required to ensure the stability of the ZIF-8 phase (either obtained by the SC or LPE approach) during the formation of the MTF layer. Moreover, the formation of ZIF-8 over the TiO2 porous films does not seem to occur either, even if the oxide is modified with APTES, highlighting the need of careful compatible interactions between the film and the MOF precursors.
As mentioned above, the use of different MOFs would endow the system with ad hoc chemical affinity, and thus is highly desirable to identify conditions for successful growth of combined MOF/MTF architectures. We have therefore explored the use of a different MOF, the Zr-based UiO-66. Differently from the single micropore size of ZIF-8, UiO-66 features two well defined micropores: a 1.1 nm wide octahedral pore and 0.8 nm wide tetrahedral pore, in a 1:2 ratio, connected by 0.6 nm wide windows.72,73 This material also differs from ZIF-8 from the fact that water is capable of accessing not only the CP of the assembled film, but also the micropores.69 Thermal and chemical stabilities of UiO-66 are also superior;58 however, synthetic conditions require the use of strong acids as modulators, and high temperatures, which might impose a limitation for the combination with MTFs.
After conducting UiO-66 synthesis on the TB 200+EE film, the critical angle corresponding to the MOF was not visible by XRR but crystals deposited onto the mesoporous film were observed by TEM and SEM (see Section S8, ESI†). However, surface coverage was somehow low in comparison with UiO-66 grown onto the bare Si substrate. Interestingly, from the analysis of the XRR pattern, it can be concluded that the accessible porosity of the TB 200+EE after MOF growth was 44%, very similar to the value corresponding to one single layer, indicating that the UiO-66 formation does not disrupt the porosity of the bottom layer (for more information see Section S10 in ESI†).
To increase the amount of UiO-66 crystals deposited onto the MTF, TB 350 was used as a base for the MOF growth. This MTF presents a higher mechanical and chemical stability, more compatible with the UiO-66 growth conditions. In this case, UiO-66 was successfully grown on it, generating the TB 350/UiO-66 bilayer. Dry- and water-saturated XRR experiments depicted in Fig. 4a revealed that not only the mesoporosity of the TB film remains accessible (30% of porosity) after the growth of UiO-66, but also that the MOF forms a layer which is also capable of water adsorption (see Section S11† for the complete XRR range). In this case, the compactness of the UiO-66 layer is relatively low, and thus the critical angle shift cannot be observed in the same way as for the other films prepared. However, it is possible to have an estimation by analysing the shift on the minimum value in the critical angle region. By doing this, a porosity accessible to water of about 9% can be estimated. Additionally, the XRD pattern shows the presence of the (111) diffraction peak of UiO-66, confirming its presence and preferred crystallographic orientation (see Section S11† for XRD in the complete range). SEM images (Fig. 4b and c), on the other hand, show a fair coverage of the TB surface with octahedrally shaped crystals of 500–600 nm size. The porosity of the TB 350 film can be seen in the SEM images with higher magnification (see Fig. S14, ESI†). As discussed above, and together with the information from micrographs, it is clear that UiO-66 is formed on top of the TB film and not extensively inside the mesopores, as in the case of ZIF-8. This is probably due to the specific interactions between MOF precursors and the TiO2 matrix.
For the inverse system, TB films were synthesised on UiO-66 as for the previous examples, thus forming the UiO-66/TB 200+EE bilayer. As can be seen in Fig. 4d, and contrary to the case of ZIF-8, a strong diffraction peak from UiO-66 was visible after formation of the MTF, thus indicating the robustness of the UiO-66 film. However, and probably due to the roughness of the system, XRR measurements could not be performed. Nonetheless, the presence of both materials was also confirmed by SEM (Fig. 4e), where a continuous MTF phase is clearly visible covering the UiO-66 crystals. As the crystals are thicker than the TB film, some cracks can be observed in the surface, exposing the mesoporous film. These results are similar to those obtained when silica particles are covered by mesoporous thin films.74 TEM images presented in Fig. 4f show that the UiO-66 crystal is clearly surrounded by the mesoporous oxide. In both configurations that combine TB films and UiO-66, the presence of MOF discrete crystals that do not completely cover the surface does not allow the determination of a single thickness for the bilayers. However, the spatial confinement of each layer is clearly demonstrated.
As mentioned before, the huge potential of this platform relies not only on the versatility rendered by the different MOFs that can be employed, but also on the fine-tuning achievable for pore sizes and the oxide employed for synthesising the MTFs. Therefore, exploring different MTFs other than TB would be of interest. Following this line of though, we have built UiO-66/MTF bilayers using the same oxide and different pore sizes (TF system, TiO2 with interpore distance in the direction perpendicular to the substrate of about 5 nm and a pore diameter around 10 nm) and a different oxide with the same interpore distance (SB, mesoporous SiO2). As shown in Fig. 5, both systems (UiO-66/TF 200+EE and UiO-66/SB 200+EE) were successfully obtained with the crystallinity of UiO-66 preserved. In both cases the mesoporous films covered the UiO-66 particles, once again with visible cracks as in the case of TB films. The porosity of the TF and SB layers is clearly distinguishable by TEM microscopy (see Fig. 5c and f); in the case of the TF system, the pores are ordered in the expected cubic structure50 while in the case of SB films the pores are locally ordered. Due to the high rugosity of the samples, a thickness cannot be defined. Moreover, XRR measurements were difficult to perform. However, for the UiO-66/SB 200+EE sample a measurement could be made, as shown in Fig. S20, ESI.† Although critical angles could not be properly determined, due to the already mentioned rugosity issues, it can be clearly seen a displacement when humidity increases, thus demonstrating the accessibility of the SB 200+EE layer.
Fig. 5 GI-XRD pattern, SEM, and TEM images for UiO-66/TF 200+EE (a–c) and UiO-66/SB 200+EE (d–f) bilayers. |
However, not all MOFs can be grown under conditions of compatibility with ordered mesoporous thin films. In particular, ZIF-8 films were not compatible and thus, stratified bilayers could not be obtained. When ZIF-8 was employed as the first layer, deposition of the MTF on top resulted in the elimination of the MOF. On the other hand, the growth or deposit of ZIF-8 on top of the MTF could not be achieved; in particular, when LPE conditions were used, the pores of the MTF were filled, affecting accessibility, which is undesirable for its use as a sensor.
The requirement of smoothness and controlled thickness remains a challenge; we have shown that while spin coating is suitable for MTFs, this is not strictly valid for the MOF layer. Although LPE synthesis of UiO-66 MOF yields reasonable smooth layers, a further degree of control is needed if multiple bilayers are to be obtained. We envision that recently proposed strategies for MOF synthesis and processing would allow this goal; e.g., the use of Zr-clusters as seeds,75 or colloidal suspensions of few-nanometer-thick MOF nanosheets obtained through doctor-blading.76 In summary, our work demonstrates that by adequately choosing the MOF identity and the deposition conditions it is possible to obtain well stratified bilayers. We have demonstrated that the combination of MOFs and MTFs constitutes a viable option for building responsive 1D-PCs with hierarchical porosity and ad hoc chemical affinity.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3ta06529d |
This journal is © The Royal Society of Chemistry 2024 |