Bharat Bhushan
Upreti
,
Navpreet
Kamboj
and
Ramendra Sundar
Dey
*
Institute of Nano Science and Technology (INST), Mohali-140306, Punjab, India. E-mail: rsdey@inst.ac.in
First published on 28th August 2023
Laser-irradiated graphene-based heterostructures have attracted significant attention for the fabrication of highly conducting and stable metal-free energy storage devices. Heteroatom doping on the graphene backbone has proven to have better charge storage properties. Among other heteroatoms, nitrogen-doped graphene (NG) has been extensively researched due to its several advanced properties while maintaining the original characteristics of graphene for energy storage applications. However, NG is generally prepared via chemical vapor deposition or high temperature pyrolysis method, which gives low yield and has a complex operation route. In this work, first a polyaniline-reduce graphene oxide (PANI-rGO) heterostructure was prepared via in situ electrochemical polymerization, followed by the deposition process. In the next step, laser-irradiation process was employed to carbonize polyaniline as well as doping of nitrogen on the graphene film, simultaneously. For the very first time, laser-irradiated carbonization of PANI on NG (cPANI-NG) heterostructure was utilized for microsupercapacitor (MSC). The as-prepared cPANI-NG-MSC shows extremely high cycling stability with a capacitance enhancement of 135% of its initial capacitance after 70000 continuous charge–discharge cycles. It is very interesting to know the origin of the capacitance enhancement, which results from the change of pyrrolic N in NG-MSC to the pyridinic and graphitic N. An on-chip NG-MSC exhibits an excellent charge storage capacitance of 43.5 mF cm−2 at a current density of 0.5 mA cm−2 and shows impressive power delivery at a very high scan rate of 100 V s−1. The excellent rate capability of the MSC shows capacitance retention up to 70.1% with the variation of current density. This unique approach to fabricate NG-MSC can have a broad range of applications as energy storage devices in the electronics market, as demonstrated by glowing a commercial red LED.
Several methods have been employed so far to synthesize N-doped graphene-based nanostructure and are classified as in situ and ex situ N-doping methods. The typical in situ N-doping procedure is a bottom-up method that generally includes chemical vapor deposition (CVD),13 arc-discharge,14 biomass pyrolysis,15 and solvothermal synthesis.16–18 However, the ex situ N-doping method includes thermal annealing,19 wet chemistry methods,20 plasma treatment,21 and ion implantation.22 The main weakness of these methods are that they either require high temperature or multistep process with hazardous reagents.23 Furthermore, low product yield, difficulties in scaling up, and insufficient N-doping make these methods unsuitable for practical applications.
On the other hand, polyaniline (PANI), an N-containing conductive polymer, has been extensively studied as an electrode material for the past few decades24 because of its facile synthesis, compelling redox properties, and moderate environmental stability. Depending on their redox state, PANI exists in different forms; most reduced pale yellow leucoemeraldine to green emeraldine salt/base and highly oxidized violet pernigraniline form.25,26 Among them, the emeraldine base form is considered to be the conductive one in its protonated state and the other two forms are insulating even after protonation.27,28 The pseudocapacitive behavior of PANI is well suited as an energy storage material, but its stability during the charge/discharge cycle is always a concern.29,30 The reasons for the unstable charge/discharge cycles are as follows: (i) ion insertion that leads to mechanical expansion, (ii) electrode material delamination, and (iii) fibrous morphology of the PANI.31 The long-term charge/discharge process leads to a volume expansion effect, which unavoidably results in the poor electrochemical stability of the supercapacitor.32,33 Moreover, PANI-based electrode materials failed to show satisfactory rate capability.34 Therefore, although PANI-based supercapacitor exhibits high specific capacitance, due to its poor rate capability and inferior cycle life, it cannot be used for commercial applications.
Therefore, to address this problem, it is necessary to develop a procedure that will give electrochemically stable PANI-graphene heterostructure with sufficient N-doping, lowered electrical resistance between PANI and graphene, as well as a sufficient diffusion channel for the electrolyte. Herein, we report a novel N-doping strategy via the in situ electrochemical polymerization of PANI in the graphene network, followed by the laser-irradiation method, encouraging the nitrogen atoms to get bonded into the graphene network and converting the rGO-PANI heterostructure into a carbonized material (cPANI-NG). In order to synthesize a comparatively less stable pseudocapacitive material PANI to a highly stable cPANI-based EDLC material, a new and efficient strategy is introduced in this work. The new strategy not only helps to improve the cycling stability of the material but also enhances the specific capacitance value of LIG. We further fabricated an in-plane microsupercapacitor with the cPANI-NG material. The resulting on-chip cPANI-NG-MSC was very efficient in showcasing the unique capacitive behavior with extraordinary cycling life. Moreover, the developed devices have been extended in series and parallel connections to make a high-voltage module that can lighten up the available red LED bulb.
Fig. 1 (a) Schematic representation of carbonization of PANI and simultaneous N-doping of graphene; (b) mechanism of electropolymerization of PANI and (c) PANI carbonization and N-doping of graphene. |
To identify the functional groups present and the degree of reduction in the different electrode materials, Fourier-transform infrared (FT-IR) spectroscopy with attenuated total reflection (ATR) technique was performed on 3rGO-PANI, cPANI-NG3, 4rGO-PANI, cPANI-NG4, 5rGO-PANI, and cPANI-NG5 samples, and the corresponding spectra are provided in Fig. S1, ESI† and Fig. 2a, respectively. The in situ polymerization of aniline under the applied potential leads to the formation of leucoemeraldine PANI, which is the reduced state of PANI.26 The band at ∼3200 cm−1 in the FT-IR spectra of xrGO-PANI in all ratios signifies the stretching frequencies for amine and –OH groups, which reduced significantly after laser irradiation.42 Two other peaks at 1720 cm−1 and 1650 cm−1 appeared in case of the 4rGO-PANI sample (Fig. 2a), which is attributed to carbonyl CO and amide peak, respectively.43,44 It should be noted here that the amide linkage between PANI and rGO is favorable only when the pH of the electrolyte solution is very low, i.e., the acidic media used for GO electrodeposition. After laser irradiation of the cPANI-NG4 sample, the intensity of the peak at 1650 cm−1 corresponding to amide linkage reduced drastically (Fig. 2a), indicating the transformation of PANi to cPANI.
Fig. 2 (a) The FT-IR spectra of 4rGO-PANI and cPANI-NG4, (b) Raman spectra of cPANI-NG3–5 and LIG samples, (c) and (d) shows N 1s and C 1s spectra of cPANI-NG4 and 4rGO-PANI, respectively. |
To understand the defect density, degree of graphitization, and crystalline nature of the samples, Raman spectroscopy was carried out for all the samples, such as LIG, cPANI-NG3, cPANI-NG4, and cPANI-NG5, as shown in Fig. 2b. The G-band positioned in the range of 1575–1585 cm−1 corresponds to E2g doubly degenerate phonons at the Brillouin zone, whereas the D-band in the range 1320–1355 cm−1 is attributed to the A1g mode, which is related to the structural disorders and defects.45 The intensity ratio of the G to D band (IG/ID) quantifies the defect density, which is directly related to nitrogen doping in LIG and the corresponding crystallite size. The IG/ID ratio was calculated for different samples and found to be 1.465 for LIG, 1.113 for cPANI-NG5, 0.943 for cPANI-NG4, and 1.180 for cPANI-NG3. The IG/ID ratio in the case of cPANI-NG4 sample confirms the formation of larger amount defects in comparison to other samples. The crystallite size was also calculated in all the samples, and the corresponding values are provided in the ESI Table S1.† The 2D-band that originates due to layered graphene-like structure almost disappeared in case of the cPANI-NG samples, which denotes the lower crystallinity of the NG samples,46 as can be observed in Fig. 2b. Moreover, the full width at half maxima (FWHM) for the Raman spectra of the cPANI-NG material broadened, which also justifies the N-doping by replacing some graphitic carbons.47,48 A slight shift of the G and D-bands in the doped graphene films towards the higher wavelength corresponds to the homogeneous incorporation of N atoms into the graphene structure at the atomic level. The degree of D and G band shifting depends on the N/C atomic ratios in the N-doped graphene film.49 This band shifting also implies the presence of some specific types of N species, such as pyrrolic, pyridinic, and graphitic N, which can serve as electron acceptors.50–52
Further, to confirm the changes in the chemical composition of the samples, X-ray photoelectron spectroscopy (XPS) was conducted, as presented in Fig. 2c and d. The full survey XPS spectra of the cPANI-NG4 sample shows C 1s, N 1s, and O 1s signals at binding energies of 285 eV, 401 eV, and 532 eV, respectively, indicating the presence of C, N, and O elements in the samples (Fig. S2, ESI†). The carbonization of PANI under laser impact leads to the N-doping, which was confirmed from the N 1s spectrum. High local temperature occurs due to photothermal reactions taking place during the laser irradiation process is responsible for more pyrrolic N after carbonization due to its greater thermal stability than the other forms of N.53 The deconvoluted N 1s spectrum of cPAN-NG4 shows that the appearance of pyridinic, pyrrolic, and graphitic nitrogen peaks corresponds to the binding energies of ∼399.5 eV, ∼401.2 eV, and ∼401.9 eV, respectively, as shown in Fig. 2c.54,55 These significant peaks for the N-doped graphene are absent but the peaks at 401.6 eV and 399.5 eV, which correspond to the Leucoemeraldine form of PANI, are present in the 4rGO-PANI film. The deconvoluted C 1s XPS spectra of cPANI-NG4 and 4rGO-PANI are shown in Fig. 2d, which clearly depicts the presence of the N–sp2-C peak positioned at a binding energy of 286.88 eV. Both the films represent the peak corresponding to the sp2-C bond, which further signifies the aromatic system of PANI and carbon graphitic structure. The peak at 288.78 eV of the 4rGO-PANI sample is assigned for –COOH, which disappeared after laser-irradiation (as shown in Fig. 2d), confirming the reduction of the sample. The deconvoluted N 1s and C 1s spectra of 3rGO-PANI, cPANI-NG3, 5rGO-PANI, and cPANI-NG5 samples are also provided in Fig. S3 and S4, ESI.† The N 1s deconvoluted spectra of cPANI-NG5 shows decreased graphitic N peak, suggesting that with increasing concentration of PANI, graphitic N decreases.
The carbonization of PANI into the graphene network develops irregular morphologies, which can be further investigated via scanning electron microscopy (SEM) and transmission electron microscopy (TEM) studies. Fig. 3a shows the SEM image of 4rGO-PANI (upper half portion) and cPANI-NG4 (lower half portion) in a same sample distinct by a yellow dotted line. The SEM images depict that 4rGO-PANI has a rough crimpled morphology, as seen in Fig. 3b and c. The sheets get flattened and linked together after laser irradiation, which can be seen in Fig. 3d and e. Still, the presence of PANI induces defects to hinder the generation of a single joint sheet as observed in the case of only laser-irradiated graphene.7 The HR-TEM studies of the cPANI-NG film in Fig. 3f shows the layered sheet structure of the as-prepared sample whereas 4rGO-PANI has few layers to multilayers sheet of large size, as seen in Fig. S5, ESI.† The TEM images reveal that after the laser irradiation, few layer graphene sheet-like structure is formed. The atomic percentages of C, O, and N are quantified using energy dispersive spectrometry (EDS) analysis in SEM, which shows that the nitrogen content is 10.3 atomic%, indicating that a sufficient amount of nitrogen has been doped on the graphene surface (Fig. S6, ESI†) compared to that of the 4rGO-PANI (Fig. S7, ESI†). The atomic percentage of nitrogen was 13.6%, suggesting that the laser irradiation has led to the removal some of the nitrogen-containing functionalities from the film. The elemental mapping of the cPANI-NG4 sample was also performed, which confirmed the homogeneous distribution of oxygen, carbon, and nitrogen throughout the sample (Fig. 3g–j). Furthermore, the selected area electron diffraction (SAED) analysis (Fig. S8, ESI†) displays the absence of lattice points characteristic to the hexagonal lattice of crystalline graphene, which indicates that the crystallinity is substantially decreased after N doping.
The electrical property study of the electrode material is very important for the electronic transport investigation. The active material must possess high electrical conductivity for its use as supercapacitor; the I–V characteristic curve shows the ohmic behavior of the films, as shown in Fig. S9, ESI.† The conductivity of the 4rGO-PANI and cPANI-NG4 films were measured by a two-probe method and calculated to be 478 S m−1 and 5933 S m−1, respectively, which is comparatively higher than that of the activated carbon (10–100 S m−1) and rGO (1000–2000 S m−1) materials. Therefore, it can be concluded that the carbonization of PANI by the LI process helps to improve the restoration of π-electron clouds and endorse fast electron transport through the cPANI-NG4 film.
A solid-state parallel linear-shaped geometry cPANI-NG4 based microsupercapacitor was designed and electrochemically characterized via different electrochemical techniques such as cyclic voltammetry (CV), galvanostatic charge/discharge (GCD), and electrochemical impedance spectroscopy (EIS) analysis. The CV curves at different scan rates (Fig. 4c) and GCD profiles at different current densities are shown in Fig. 4c and d, respectively. The EDLC behavior of the CV curve in Fig. 4c indicates that most of the PANI polymers are carbonized in the film or get fused with the graphene layer or form N-doped graphene. PANI is an electroactive conducting polymer, which shows pseudocapacitive response (Fig. S10, ESI†), but after the LI process, its carbonized form displays electric double-layer capacitor (EDLC) type behavior, demonstrating superior charge storage property of the material. The CV curve at different scan rates from 10 to 100 mV s−1 shows perfect rectangular shape, retaining the EDLC behavior of the film (Fig. 4c). Fig. 4d illustrates the GCD profile of the device with varying current density from 10 to 0.25 mA cm−2. The specific capacitance (Csp) of the device was calculated from the GCD curve and found to be 43.5 mF cm−2 at a current density of 0.25 mA cm−2. The electrochemical impedance spectroscopy (EIS) measurement was carried out to further understand the ease of ionic transport and capacitive nature of the device in the frequency range of 0.01 Hz to 100 kHz at an AC amplitude of 0.5 V. The Nyquist plot with its fitted curve (inset shows corresponding Randles Equivalent Circuit) shows a vertical line almost parallel to the Y-axis in the lower frequency region, which demonstrates perfect double layer formation by the cPANI-NG-MSC device (Fig. 4e). The parameters of the Randles circuit determined by the curve fitting of Nyquist plot are mentioned in Table S2, ESI.† The maximum area normalized energy density (EA) and power density (PA) of the cPANI-NG-MSC were calculated to be 1.95 m Wh cm−2 and 4.96 W cm−2, respectively and the corresponding Ragone plot for the device is provided in Fig. S11, ESI.†
Generally, the specific capacitance of a supercapacitor decreases with increasing scan rate or increasing current densities, causing poor rate capabilities. The rate capability of the prepared cPANI-NG4-based MSC was determined with the capacitance retention vs. current density plot for cPANI-NG4 at 0.25–10 mA cm−2. The retention of the Csp was 70.1% of its initial capacitance value (Fig. 4f). The rate capability of the MSC was further evaluated by operating CV from 200 mV s−1 to 500 V s−1, as shown in Fig. 5a–f. The rectangular shape of the device was retained even at a very high scan rate of 100 V s−1 (Fig. 5e), indicating excellent power delivery of the device. There is a little distortion in the shape of the voltammogram at 500 V s−1, as shown in Fig. 5f. This study shows the fast formation of the adsorption layer on the surface of the film; as a result, instantaneous power delivery can be obtained.
Fig. 5 CV curves of cPANI-NG-MSC at different scan rates (a) 200 mV s−1, (b) 500 mV s−1, (c) 1 V s−1, (d) 10 V s−1, (e) 100 V s−1, and (f) 500 V s−1, respectively. |
The cycling stability is another one important factor of the energy storage system for the commercial feasibility of the device. The cycling performance of the device was examined under continuous long-term charge–discharge (CD) cycles. Generally, pseudocapacitive material such as PANI shows the degradation of the capacitance in the longer period CD cycles as the polymer contraction and expansion weakens the charge storage tendency of the material.33 The cycling performance of the cPANI-NG MSC was examined using the galvanostatic charge–discharge cycling in the potential window of 0–1 V at a current density of 2 mA cm−2 for 70000 continuous cycles, as shown in Fig. 6a. The inset of the Fig. 6a shows the retained triangular CD profile in different time intervals, showing the extraordinary stability of the cPANI-NG-MSC device in long run cycling. Interestingly, the device preserved almost 100% of coulombic efficiency during the cycling. It is stimulating to note that the MSC device shows an increase in the specific capacitance of up to 135% of the initial capacitance value after 70000 cycles. The enhancement in the capacitance value after cycling can be explained by considering the nature of doped-nitrogen present in the laser-irradiated N-doped graphene film. In case of N-doped graphene, the total capacitance is obtained from the contribution of electric double layer capacitance (CEDL) and the quantum capacitance (Cq). Ignoring the polarization effect of the electrode surface, the quantum and EDL capacitance can be considered separately for studying the total capacitance.58–60 Amongst the different forms of N present in the material, namely, graphitic, pyridinic, and pyrrolic, graphitic and pyridinic nitrogen enhance the total capacitance by increasing the quantum capacitance, whereas the pyrrolic nitrogen limits the increase in total capacitance.61 In this case, we observed that the enhancement in Csp is up to 50000 cycles, and the Csp was stable up to 70000 cycles. This enhancement corresponds to the decrease in the pyrrolic N present in the sample and enhancement of the pyridinic and graphitic N during GCD cycling. To prove this, XPS study was performed with the sample before and after the cycling test. The XPS study reveals that the area under the curve for pyrrolic N is more in comparison to the pyridinic and graphitic N for the sample before stability, whereas the same is decreased after stability, and the intensity of pyridinic N is increased after stability, as shown in Fig. 6b–d. The CV plot at 100 mV s−1 of cPANI-NG4 before and after cycling stability is shown in Fig. S12, ESI.† As expected, the area under the curve after cycling stability is greater than the initial capacitance, which is due to increased capacitance value during cycling, corroborating the results obtained from the GCD study.
In order to meet the commercial requirement for current and/or voltage output, it is necessary to check the response of MSC devices in-series and in-parallel connection. Identical cPANI-NG4 MSC devices are connected in series and parallel combination in order to meet the energy and power density requirement of the device. The MSC devices connected in series show increment in the operating voltage from 1 V to 2 V and 3 V when two and three devices are connected in series configuration, respectively. However, as expected, when the devices are connected in parallel, a stepwise increment in the output current is observed. The GCD profile and CV plots of series and parallel connections of the devices are represented in Fig. 7. Fig. 7a shows the GCD profile with the increasing series connections of the devices, which shows the increase in the cell voltage up to 3 V, and the corresponding CV curves for the series combination is given in Fig. 7b. The three devices in series combination were extended in the parallel configuration as 3S × yP, where y = 1, 2, 3. The CV and GCD curves for different series and parallel configurations of devices is shown in Fig. 7c and d, and the corresponding digital image is shown in Fig. 7e. A comparative tabular representation with different parameters of our work and other reported works involving PANI and graphene (or carbon)-based MSCs is given in Table S3, ESI.† The comparison shows the superiority of the cPANI-NG material other than PANI-based supercapacitors. To demonstrate the use of cPANI-NG-MSC for commercial purpose, the ability of the device was validated by glowing a commercial LED. The MSC devices was patterned in 3S × 2P (Fig. 7e) configurations and was fully charged to 3 V for 3 minutes using a commercial DC power supply source, as shown in Fig. 7f. The module can lighten up a commercial 1.5 V LED, demonstrating the practical viability of the homemade in-plane microsupercapacitor.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3nr02862c |
This journal is © The Royal Society of Chemistry 2023 |