Open Access Article
Bin
Wu
ab,
Haibing
Meng
c,
Dulce M.
Morales
de,
Bo
Liu
f,
Deniz
Wong
g,
Christian
Schulz
g,
Giacomo
Zuliani
d,
Maddalena
Zoli
d,
Omeshwari Y.
Bisen
d,
Samuel
Hall
h,
Annika
Bande
hi,
Zhenbo
Wang
f,
Marcel
Risch
d and
Tristan
Petit
*a
aNanoscale Solid-Liquid Interfaces, Helmholtz-Zentrum Berlin für Materialien und Energie GmbH, Albert-Einstein-Straße 15, 12489 Berlin, Germany. E-mail: tristan.petit@helmholtz-berlin.de
bInstitute of Physics, Humboldt University Berlin, Newton-Straße 15, 12489 Berlin, Germany
cCollege of Chemistry, Taiyuan University of Technology, 030024 Taiyuan, China
dNachwuchsgruppe Gestaltung des Sauerstoffentwicklungsmechanismus, Helmholtz-Zentrum Berlin für Materialien und Energie GmbH, Hahn-Meitner-Platz 1, 14109 Berlin, Germany
eEngineering and Technology Institute Groningen (ENTEG), University of Groningen, Nijenborgh 3, Groningen, 9747 AG, Netherlands
fMIIT Key Laboratory of Critical Materials Technology for New Energy Conversion and Storage, School of Chemistry and Chemical Engineering, State Key Laboratory of Space Power-Sources, Harbin Institute of Technology, 150001 Harbin, Heilongjiang, China
gDepartment of Dynamics and Transport in Quantum Materials, Helmholtz-Zentrum Berlin für Materialien und Energie GmbH, Albert-Einstein-Straße 15, 12489 Berlin, Germany
hTheory of Electron Dynamics and Spectroscopy, Helmholtz-Zentrum Berlin für Materialien und Energie GmbH, Hahn-Meitner-Platz 1, 14109 Berlin, Germany
iInstitut für Anorganische Chemie, Leibniz Universität Hannover, Callinstr. 9, 30167 Hannover, Germany
First published on 28th May 2025
Non-noble metal electrocatalysts for the oxygen reduction reaction (ORR) are urgently needed in metal–air batteries, seawater batteries and fuel cells. Fe–N–C materials are among the most active catalysts for the ORR. Fe–N–C synthesis usually requires post-heat treatment after pyrolysis which is time-consuming and inevitably triggers inactive aggregate Fe species due to difficulties in controllable atom-level modulation. Here, highly active Fe–N–C catalysts were prepared by a simple process involving an ammonia etching treatment by using ZIF-8 as a hard template and a mixture of FeSO4 and 2-methylimidazole as the Fe, N and C precursors. The direct ammonia treatment modulates N and Fe active species and removes the unstable carbon framework to form pyrolyzed Fe–N–C nanocages with a well-dispersed pore structure. The obtained Fe–N–C exhibits a potential of 0.89 V vs. RHE at a kinetic current density of −1 mA cm−2 (E−1) for the ORR, similar to commercial Pt/C, but outperforming it in terms of stability and methanol tolerance. In situ electrochemical Raman and density functional theory provide insights into the origin of the activity of Fe–N–C materials and the underlying ORR electrocatalytic mechanisms at the molecular level.
Within the preparation of Fe–N–C catalysts, annealing in ammonia is often used to either form active sites15 or to improve catalytic performance.11 As confirmed by several studies, using an Fe precursor with a high iron content during a pyrolysis step in an argon atmosphere prevents a well-dispersed atomic dispersion of iron (FeN4 formation) and thus leads to a lower catalytic activity.15 In contrast to pyrolysis in Ar, an additional heat treatment in NH3 afterward increases the absolute amount of Fe in FeN4 coordination.11,15 Moreover, NH3 etching can modulate Fe–Nx active sites by forming different N species.15 However, while enhancing the performance of Fe–N–C catalysts, post-heat treatment after pyrolysis is time-consuming and inevitably gives rise to a non-uniform structure.16 Moreover, a secondary heat treatment after pyrolysis probably conducts the formation of a carbon framework rich in disordered micropores, which are hardly accessible and lead to the inhomogeneous distribution of active sites, thus hindering optimization of activity due to steric hindrance and the large mass transport resistance.17
In this study, a Fe–N–C material was synthesized via an ammonia etching strategy by using ZIF-8 as the hard template and a mixture of FeSO4 and 2-methylimidazole as the Fe, N and C precursors. Exposure to ammonia was correlated with the modulation of N and Fe active species and removal of the unstable carbon framework to form well-dispersed pore structures in the pyrolyzed Fe–N–C catalysts. The Fe–N–C catalyst is far superior to the N–C species in catalyzing the ORR, although their N content is quite similar, demonstrating the dominant role of the Fe–N4 active site over N4–C species. Both the ordered mesoporous structure of the carbon framework and the FeN4 active site along with small clustering of Fe are confirmed with X-ray diffraction (XRD), X-ray absorption spectroscopy (XAS) and aberration-corrected high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM). This work provides a new strategy for effectively manipulating the ORR electrocatalytic performances of Fe–N–C materials by direct NH3 etching for a sustainable energy conversion system.
:
1 volume ratio) in the presence of 2 vol% Nafion solution (∼5% Nafion in a mixture of alcohols, Sigma-Aldrich). The total catalyst loading on the GC electrode was 200 μg cm−2. The electrochemical experiments were conducted in O2-saturated or Ar-saturated 0.1 M KOH solution and 0.5 M H2SO4 solution (Sigma-Aldrich) at room temperature after purging the electrolyte with Ar or O2 for 30 min. For each sample, three freshly prepared electrodes were measured under the same conditions to assess the reproducibility of the measurements.
Prior to the ORR activity characterization, 10 cyclic voltammograms (CVs) were recorded at a scan rate of 100 mV s−1 in the potential range from 0.2 to −0.4 V vs. Hg|HgO|NaOH and no change of the voltammetric response was observed during the last CVs. Subsequently, electrochemical impedance spectra were collected in the frequency range from 100 kHz to 1 Hz with an AC amplitude of 10 mV (RMS) to determine the uncompensated resistance (Ru) and later correct the measured data (Emeasured) by the iRu-drop according to eqn (1), where imeasured is the measured current. All potentials were converted to the reversible hydrogen electrode (RHE) scale by measuring the voltage between an RHE electrode (Gaskatel) and the reference electrode for 10 min at the beginning of each measurement day. The last value recorded (VRE) was applied to calculate the potentials vs. RHE according to eqn (1) each measurement day. The average value obtained for different experiment days was 0.87 ± 0.01 V. The obtained Ru values were on average 74.9 ± 3 Ω for all samples.
| Ecorrected = Emeasured + VRE − imeasuredRu | (1) |
To investigate the ORR stability, 100 CVs were recorded with the catalyst-modified electrodes at a scan rate of 50 mV s−1 in the potential range from 0.2 to −0.8 V vs. Hg|HgO|NaOH reference electrode at a rotation rate of 1600 rpm. The current densities at 0.5 V vs. RHE were then extracted at different cycling rates and plotted as a function of the corresponding number of cycles.
The CH3OH tolerance tests were carried out by chronoamperometric measurements at 0.45 V vs. RHE in an O2-saturated 60 mL 0.1 M KOH electrolyte. After 240 s, the measurement was paused to inject 0.5 M CH3OH (1.22 mL) into the electrochemical cell and the solution was mixed with a magnetic stirrer without disassembling any cell component. The chronoamperometric measurement was then resumed for 240 s more.
The electrochemical double layer capacitance was estimated from the CVs in the non-faradaic potential window from 0.2 to −0.4 V vs. Hg|HgO|NaOH at various scan rates (10, 25, 50, 75, 100 and 150 mV s−1). The fitting model is based on an allometric regression with the variables Y and X as the current and the scan rate, respectively.22 The slope b corresponds to the capacitance while an exponent α is associated with compensating deviations from linearity (eqn (2)).22
| Y = bXα | (2) |
| 1/J = 1/(0.62nFC0D02/3V−1/6ω1/2) + 1/JK | (3) |
485 C mol−1), C0 is the bulk concentration of O2 (1.2 × 10−6 mol cm−3), D0 is the diffusion coefficient of O2 in 0.1 M KOH (1.9 × 10−5 cm2 s−1), V is the kinematic viscosity of the electrolyte (0.01 cm2 s−1), ω is the angular velocity of the disk electrode, and JK is the kinetic-limited current density.23 The kinetically controlled potential region is defined here by the potential region at which the current density remains below 20% of the limiting current density.
A rotating ring disk electrode (RRDE) consisting of a GC disc (∅ = 4 mm, 0.126 cm2) and a concentric platinum (Pt) ring (∅ = 7 mm, 0.188 cm2) in polyether ether ketone was used as the working electrode (WE). The GC/Pt-RRDE was polished using deagglomerated alumina (Al2O3) pastes with particle sizes of 0.05 μm. The electrode was sonicated in 18 MΩ water after the polishing steps. LSV was performed in an O2-saturated 0.1 M KOH electrolyte using the RRDE to calculate the collection rate, electron transfer number, and yield of intermediate HO2−. The disk potential is scanned from 1.2 to 0.0 V (vs. RHE), and the platinum ring potential is fixed at 1.2 V vs. RHE with a rotation speed of 1600 rpm at a sweep rate of 5 mV s−1. The ring electrode potential is higher than the disk electrode potential to collect the signal of hydrogen peroxide oxidation. The ring electrode potential of 1.2 V vs. RHE can ensure the oxidation of hydrogen peroxide ions diffusing from the disk electrode to the ring electrode.
The hydrogen peroxide yield and the electron transfer number (n) were calculated with the following eqn (4) and (5) assuming the absence of any side reactions:
| H2O2 (%) = 200 × (IR/N)/(ID + IR/N) | (4) |
| n = 4 × (ID)/(ID + IR/N) | (5) |
S
O stretching of sulfate is also revealed by the bands at 1104 cm−1 while the band at 612 cm−1 corresponds to S–O stretching in FeSO4·7H2O.28 These two characteristic peaks related to SO42− of FeSO4·7H2O are not present in Fe-ZIF-8, indicating that the Fe species in this material is not in the form of sulfate salt. The sharp peaks at around 422 cm−1 and 688 cm−1 corresponding to the stretching vibration of Zn–N bonds formed between zinc and imidazole can be observed in the two cases,29 suggesting that the incorporated Fe species are not substituting Zn in the ZIF structure. Furthermore, the characteristic peaks in the range of 700–1600 cm−1 originating from the stretching vibration of the 2-methylimidazole ligands only can be seen in Fe-ZIF-8 and ZIF-8, and the stretching vibration peak of the C
N bond in the imidazole ring appears at 1585 cm−1 of Fe-ZIF-8 and ZIF-8, indicating that Fe doping does not cause the disappearance of organic ligands.30 The rigid structure of ZIF-8 nanocages can reduce the Fe species from aggregation during the heat treatment at high temperatures.
Several characterization techniques were used to confirm the chemical structure and morphology of the Fe–N–C catalyst. Scanning electron microscopy (SEM) images of Fe–N–C NH3 (Fig. 2a), Fe–N–C Ar (Fig. S3a†), and NC (Fig. S4a†) samples demonstrate that after heat treatment, Fe–N–C samples and NC (prepared by skipping the step involving the Fe precursor during the synthesis) retain their initial dodecahedral shape while the surface becomes rougher. In the transmission electron microscopy (TEM) images (Fig. 2b and c) of Fe–N–C NH3, there are no nanoparticles or nanoclusters observed over the entire carbon matrix and the images demonstrate a dodecahedral shape as well. The Fe–N–C Ar and pure NC exhibited the same morphology as Fe–N–C NH3 as shown in Fig. S3 and S4.†Fig. 2d shows the aberration-corrected high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) image of Fe–N–C NH3. Single-site iron atoms are clearly identified by isolated bright dots marked with red circles, indicating that single metal sites were uniformly distributed in the carbon skeleton matrix. Similar observations for Fe–N–C Ar are shown in Fig. S3.† Selected-area electron diffraction (SAED) patterns of Fe–N–C NH3 (Fig. 2e) and Fe–N–C Ar (Fig. S3e†) display clear crystalline diffraction rings corresponding to the (100) and (002) facets of the carbon matrix.31 This demonstrates the formation of mostly single atom structure in Fe–N–C materials, and agrees well with the XRD pattern. In addition, energy-dispersive X-ray spectroscopy (EDS) mapping images exhibit that Fe, N, and C are uniformly distributed on the whole architecture of Fe–N–C samples (Fig. 2 and S3†). There is no Fe distribution in the carbon matrix of pure NC as shown in Fig. S4.† Small traces of Zn are homogeneously detected over the whole sample (Fig. S5†). These results demonstrate at well-dispersed structures derived from the pyrolysis of ZIF-8 under NH3 and Ar could serve as an excellent matrix to host atomically dispersed Fe-based active sites and thus maximize the density of single-atom catalytic sites. Knowing the limitation of TEM in terms of resolving single atoms and signals from a very small area of scanning, XAS studies were performed to further understand the distribution in the N-doped carbon matrix which is discussed later.
From the XRD patterns obtained with the annealed samples (Fe–N–C NH3, Fe–N–C Ar and NC, Fig. 3a), two broad diffraction peaks at 25° and 43° indexed to the (002) and (100) planes of the N-doped graphitic carbon can be observed for all three samples.32 No clear differences were found between samples annealed under NH3 and Ar, both presenting amorphous and graphitic carbon characteristic peaks. Raman spectra were collected for the same three samples and are shown in Fig. 3b. The spectra exhibit two peaks at 1347 cm−1 (D band) and 1591 cm−1 (G band) with an intensity ratio (ID/IG) of 1.00 for all samples, indicating a similar degree of graphitization.33 The pore properties were analysed by nitrogen adsorption/desorption isotherms. The pure NC has a significantly larger specific surface area (497 m2 g−1) than Fe–N–C NH3 (380 m2 g−1), Fe–N–C Ar (345 m2 g−1) and Pt/C 20% (131 m2 g−1). As shown in Fig. 3c, all samples displayed type IV isotherms with a steep increase in Vads at relatively low N2 pressures (P/P0 = 0–0.015) due to micropores and a well-defined hysteresis loop at higher N2 pressures (P/P0 = 0.45–0.95) due to mesopores. Such a mesoporous structure can be further verified by the pore size distribution plots in Fig. 3d. The Fe–N–C NH3 and pure NC samples showed a very similar pore distribution with an average pore size of ≈3.5 nm, while Fe–N–C Ar demonstrated an average pore size of ≈3 nm.
![]() | ||
| Fig. 3 (a) XRD patterns, (b) Raman spectra, and (c) N2 adsorption–desorption isotherms with (d) corresponding pore size distributions of Fe–N–C NH3, Fe–N–C Ar, NC and Pt/C 20%. | ||
X-ray photoelectron spectroscopy (XPS) allows the identification of the binding states of Fe, N, and C in the Fe–N–C catalyst, as shown in Fig. 4, 5 and S6.† The presence of Fe is identified in the survey spectrum of Fe–N–C (Fig. S6a†) and represents less than 1 at% (Table S1†). The nitrogen (oxygen) content of Fe–N–C NH3 is 7.1 (9.7) at%, while those of Fe–N–C Ar and pure NC are 7.4 (6.5) at% and 6.3 (6.3) at%, respectively. The highest O contents of Fe–N–C NH3 can be ascribed to a higher density of oxygen defects.34 Some residues of Zn (∼0.1 wt%) are identified in Fe–N–C NH3 and NC as evidenced by the Zn Auger peak at 499.4 eV and Zn 2p peaks from 975 to 1046 eV. The C 1s XPS spectra (Fig. 4a, c and e) of Fe–N–C NH3, Fe–N–C Ar and pure NC can be deconvoluted into three peaks at around 284.3 eV, 285.3 eV, and 289 eV, attributed to C–C, C–N and C
O, respectively. Meanwhile, the component C–N of Fe–N–C NH3 exhibits a slight shift to higher energy compared to Fe–N–C Ar, suggesting a lower electron cloud density and thus a higher electron transfer from Fe to the N-doped graphitic matrix at the Fe–N–C NH3 interfaces.35 N-doping in carbon can change the charge or spin distribution, which facilitates the O2 adsorption and thus is expected to enhance the ORR performance.34,35 The N 1s XPS spectra of the three catalysts reveal three dominant peaks at around 398.2 eV, 400.2 eV and 403.8 eV, assigned to pyridinic N, pyrrolic N or pyridonic (N adjacent to a C–O group), and oxidized N, respectively, as shown in Fig. 4b, d and f. Note that defective sites related to C–O and C–N at the C 1s and pyrrolic and oxidized N in the N 1s exhibit broader peaks than the C–C and pyridinic N components (Table S2†), which are mostly related to the well-defined graphitic carbon and Fe–N–C active sites. The broadening is most likely related to slight chemical shifts due to the different chemical environment that cannot be resolved by XPS. The content of pyridinic N in Fe–N–C NH3, Fe–N–C Ar and pure NC is 35 (±2) % while the content of pyrrolic N is 57% in Fe–N–C NH3, 54% in Fe–N–C Ar and 53% in pure NC as summarized in Table S2.† The amount of pyrrolic/pyridonic N in Fe–N–C NH3 and Fe–N–C Ar is therefore increased compared to the pure NC, which instead presents more oxidized N. Pyridinic and pyrrolic N sites are believed to be beneficial for ORR chemistry due to improved oxygen adsorption resulting from a weak bonding energy of oxygen molecules.34 In addition, O 1s XPS spectra confirm the existence of C–OH as shown in Fig. S6b–d,† which is in line with C 1s XPS spectra. Moreover, the peak at around 531.5 eV can be assigned to C
O bonds, suggesting the possible presence of pyrrolic-like nitrogen groups, which were shown to play a role in the ORR of metal-free catalysts.36 The C–OH and C
O groups represent roughly 18% and 82% of the XPS O 1s based on the fitting results (Table S2†), which are related to ∼1.7 at% and 8 at%, respectively for Fe–N–C NH3. C
O bonds are probably not situated close to Fe4N sites as they would lead to strong distortion of the carbon framework. On the other hand, C–OH groups may be stable near the active sites for the ORR and affect the catalytic activity, and it will be discussed in the following sections based on DFT calculations. N
O bonds coming from oxidized nitrogen detected at the N 1s may also contribute to this peak.37 From the XPS Fe 2p spectra in Fig. 5a, both Fe–N–C NH3 and Fe–N–C Ar exhibit similar compositions with Fe 2p3/2, Fe(II) satellite and Fe 2p1/2 components, respectively.38,39 Notably, the Fe 2p XPS spectrum of Fe–N–C NH3 appears at lower binding energy than that of Fe–N–C Ar, which may be related to the presence of slightly more oxidized Fe atoms in the Fe–N–C Ar catalyst.
The X-ray absorption (XA) spectra at the Fe L-edge of Fe–N–C NH3 and Fe–N–C Ar are shown in Fig. 5b. This indicated the signature of Fe moieties with an oxidation state close to +3. The Fe3+ features are related to the Fe–N bonds, with an L3-edge composed of two peaks resulting from ligand field splitting. Similar features appear in Fe-doped carbon nanotubes and polymeric carbon nitride.40,41 The weak shoulder at 713.1 eV may be related to a charge transfer state resulting from the hybridization with oxygen atoms, and possibly nitrogen atoms.42 The Fe L3-edge resonant inelastic X-ray scattering (RIXS) spectra of Fe–N–C NH3 were also recorded at selected photon energies corresponding to the main XA features and are plotted as a function of the energy loss (Fig. 5c). Two energy loss features at 1.3 eV (A) and 2.6 eV (B), attributed to d–d excitations, are detected for excitation energy below the main L3 peak.42,43 Peak A is most clearly observed around 708.4 eV, whereas peak B is more intense at 709.6 eV excitation energy. When the incident energy is detuned above the L3 resonance (713.1 eV), a broad band around 5 eV is observed, which is related to transitions from 3d to 2p states localized at the Fe atom,44 but could also potentially result from the hybridization with the nitrogen ligand. The Fe L3-edge RIXS of Fe–N–C Ar in Fig. 5d also shows the same features as that of Fe–N–C NH3, suggesting a similar chemical environment of Fe atoms in both materials. This RIXS signature supports the fact that Fe atoms are incorporated in the N-doped carbon matrix with an oxidation state close to +3. Fe–N–C active sites with a high Fe oxidation state were found to increase ORR activity compared to Fe with an oxidation state closer to +2.45
The bulk sensitive XA spectra at the Fe K-edge of Fe–N–C NH3 and Fe–N–C Ar were obtained. Fig. 5e shows the X-ray absorption near-edge structure (XANES) spectra of Fe–N–C NH3 and Fe–N–C Ar along with reference samples Fe3O4 and Fe2O3 and iron phthalocyanine (FePc). The edge position of Fe–N–C NH3 and Fe–N–C Ar (Fe K-edge at 0.5 of normalized absorption intensity) is overlapped with the Fe2O3 reference sample, indicating the bulk oxidation state close to +3, which is well aligned with XAS at the Fe L3 edge and RIXS analysis. The local structure around the absorbing atom in Fe–N–C NH3 and Fe–N–C Ar was further tracked by EXAFS at the Fe K-edge (Fig. 5f). The Fourier transform (FT) of the EXAFS spectra of Fe–N–C NH3 and Fe–N–C Ar showed multiple peaks, which did not support a pure single-site phase. The distinct peak for Fe–N around 1.5 Å reduced distance was clearly observed in Fe–N–C NH3 and Fe–N–C Ar, confirming the presence of Fe–Nx coordination.46 We note that the FT of FePc showed a peak at 2.46 Å reduced distance which had been assigned to Fe–C bonds.47 The FT peaks in our samples were clearly distinct. The second coordination peak in Fe–N–C NH3 overlaps with that of the Fe metal foil at 2.2 Å reduced distance, suggesting the presence of Fe–Fe bonding along with single atom sites.48 Meanwhile, in Fe–N–C Ar a small peak around 3.0 Å reduced distance coincided with the second coordination peak of Fe3O4 reference oxides,49 which suggests the presence of small metal oxide nanoparticles along with Fe–Nx sites. Overall, both Fe–N–C NH3 and Fe–N–C Ar exhibited single atom sites along with small Fe metal clusters on Fe–N–C NH3 and FeOx nanoparticles on Fe–N–C Ar.
Profiting from a series of merits, such as rich defects and a high total content of nitrogen and oxygen species as well as large specific surface area, Fe–N–C catalysts (both Fe–N–C NH3 and Fe–N–C Ar) display extreme hydrophilicity with a contact angle (θ) of approximately 0°, much better than pure NC (15°) and commercial Pt/C (150°) (Fig. S7†). The favourable hydrophilicity has been proven to increase the transport and adsorption of hydrated O2 to the active sites, further improving ORR activity.34,35 While this may have a relatively small impact on half-cell performances, it may impact more significantly full membrane electrode assembly.
The diffusion-limited current density JL (determined here at a potential of 0.2 V vs. RHE) of Fe–N–C NH3 (−5.9 ± 0.06 mA cm−2) is comparable to that of commercial Pt/C 20% (−5.8 ± 0.1 mA cm−2), and higher than that of Fe–N–C Ar (−5.5 ± 0.08 mA cm−2) and pure NC (−4.6 ± 0.07 mA cm−2), which could be correlated to differences in selectivity between these materials. To gain further insight into the electron-transfer pathway of all samples, the RDE measurements were conducted at various rotation speeds from 100 to 1600 rpm.54 The measurements show again a high reproducibility (Fig. S9†). Fig. 6b and S10a, c and e† show that the current densities were enhanced with the increasing rotation speed, while the onset potentials remained constant at different rotation speeds. Fig. 6c and S10b, d, f† illustrate the Koutecký–Levich (K–L) plots of all samples, which displayed excellent linearity between the inverse of the current density (1/j) and the negative of the square root of the scan rate (ω−0.5) at different potentials. Moreover, the numbers of transferred electron per oxygen molecule in the ORR of Fe–N–C NH3 were almost the same between 0.625 and 0.75 V vs. RHE, implying first-order reaction kinetics for the ORR.55 The transfer numbers of these three catalysts are estimated to be 3.54 (pure NC), 3.95 (Fe–N–C Ar) and 3.98 (Fe–N–C NH3) from the slopes of the linear fitting plots. The values of the Fe–N–C samples approach n = 4, corroborating a four-electron oxygen reduction process (Fig. 6c and S10†).
The correlation between specific surface area and electrochemically active surface area (ECSA) is highly important to confirm the extent of the surface area involved in the electrochemical reaction.56 Specific surface area refers to the total surface area of a material per unit mass or volume, while ECSA refers to the portion of the surface area that is electrically conductive and exposed to the electrolyte.57,58 Since the electrochemical reactions, including the ORR, take place at the interface between the electrode and the electrolyte, a larger ECSA indicates higher availability of catalytic sites and better conductivity. Therefore, we used the non-faradaic capacitive double-layer current as a proxy of the ECSA to further evaluate the relative catalyst activity of the materials in this study. It was measured using the scan-rate dependence of cyclic voltammograms (CVs).57,58 For this purpose, CVs were collected with each of the catalysts at scan rates ranging from 10 to 1000 mV s−1 in the non-faradaic potential range between 0.9 and 1.1 V vs. RHE for Fe–N–C NH3, Fe–N–C Ar and pure NC. The obtained voltammograms are shown in Fig. 6d, S11a, c and e† for Fe–N–C NH3, Fe–N–C Ar, pure NC and Pt/C 20%, respectively. From the obtained voltammograms, the anodic and cathodic currents measured at a potential of 1.0 V vs. RHE for Fe–N–C NH3, Fe–N–C Ar and pure NC were extracted and plotted as a function of the scan rate as shown in Fig. 6e, S11b and d,† respectively. The double-layer capacitance (Cdl) values can be calculated by determining the slope using an allometric fit according to a previously reported procedure (fitting details are shown in Table S3†).22 As shown in Fig. 6f, the average Cdl is 0.92 mF for Fe–N–C NH3, higher than that of Fe–N–C Ar (0.37 mF) and pure NC (0.62 mF), indicating the higher electrochemical active surface area of the Fe–N–C NH3 catalyst among N–C materials, which is attributed to the large surface area and defective network of the Fe–N–C NH3 catalyst, elucidating numerous active site exposure and thus profiting mass transfer and charge transport during the ORR. It is noted that the specific surface areas of Fe–N–C NH3 and Fe–N–C Ar are very similar whereas the average Cdl and expected ECSA of Fe–N–C NH3 are much higher than those of Fe–N–C Ar, indicating that a larger portion of the surface area in Fe–N–C NH3 is in electrochemical contact with the electrolyte compared to Fe–N–C Ar, leading to relatively superior ORR performance.
Additionally, long-term stability and methanol tolerance are two other critical factors for application in fuel cells.59 Thus, we examined the stability through recording 100 CVs and then extracted the current at 0.5 V vs. RHE of Fe–N–C NH3, Fe–N–C Ar and Pt/C 20% (Fig. 7a and S12a and b†). Fig. 7b shows the currents recorded with the different samples as a function of the cycle number, relative to the current recorded during the first cycle. Fe–N–C NH3 had the best durability with almost 99.4% of the current maintained in the system by the end of the test compared to that of Fe–N–C Ar (96.8%) and commercial Pt/C (98.2%). In addition, methanol tolerance was measured by i–t chronoamperometric response under the same conditions with the addition of 0.5 M methanol. As shown in Fig. 7c, the current density of Pt/C dropped sharply. In contrast, it recovered rapidly after a tiny transitory disturbance for Fe–N–C NH3 and Fe–N–C Ar, indicating the superb methanol tolerance ability of Fe–N–C materials.53 After recording 100 cycles for the stability test and 6-min methanol tolerance test, LSVs were recorded to compare the activity before and after the stability and methanol tolerance test. As shown in Fig. 7d and S12c and d,† negligible negative shifts were detected for the E−1 and Eonset of Fe–N–C NH3, while a 40 mV loss for E−1 of Pt/C 20% and a large decline for JL of Fe–N–C Ar were observed, indicating that Fe–N–C NH3 had a better stability than other catalysts. Also, LSV curves of Fe–N–C NH3, Fe–N–C Ar and Pt/C 20% were obtained before and after the methanol tolerance test (Fig. 7d and S12c and d†); Pt/C 20% and Fe–N–C Ar produced an obvious oxidation peak of methanol in the LSV curve and a large potential loss of 25 mV with a large decrease of JL,0.2, respectively, while the E−1 of Fe–N–C NH3 has only a slight 10 mV positive shift compared to its LSV curve before the methanol tolerance test. These results indicate that Fe–N–C NH3 has the best durability and tolerance to methanol compared with commercial Pt/C and Fe–N–C Ar. Longer stability tests on real fuel cells will be needed to assess the potential of Fe–N–C NH3 for practical applications.
To further evaluate the ORR efficiency, an electrocatalytic experiment using a rotating ring disk electrode (RRDE) was carried out in O2-saturated 0.1 M KOH aqueous solution. The potential of the Pt ring on the RRDE was set as at 1.2 V vs. RHE during the ORR test to monitor the concentration change of HO2−. The ring current density of both Fe–N–C NH3 and Pt/C 20% are lower compared to disk counterparts, indicating a low amount of HO2− formation (Fig. 7e). As shown in Fig. 7f, the yield of HO2− remains below 3% over the potential ranging from 0.2 to 0.8 V vs. RHE. Moreover, the average numbers of electron transfer (n) for Fe–N–C NH3 and Pt/C 20% are 3.98 and 3.97 from 0.2 to 0.8 V vs. RHE, leading to the average yield of HO2− being strikingly suppressed to average 1.3% and 1.6%, respectively. This result highly supports the calculation results derived from K–L plots, confirming that the Fe–N–C NH3 electrode advances a four-electron ORR process as commercial Pt/C 20%. Thus, the low production of peroxide is evidence of a four-electron ORR pathway over the Fe–N–C NH3 electrode, indicating enhanced catalytic efficiency. The ORR performance in terms of the activity and number of electrons transferred of recently reported PGM-free Fe-based catalysts is listed in Table S4,† demonstrating the excellent ORR catalytic performance of Fe–N–C NH3 materials.
![]() | ||
| Fig. 8 In situ Raman measurements at applied potentials (vs. Ag/AgCl) for the Fe–N–C NH3 electrocatalyst in 0.1 M KOH during the ORR process. | ||
| Eads = Esystem − (Eclean + Emolecule) |
The results for the addition of up to 4 OH groups for each of the three ORR structures are shown in Fig. 9b. For an increasing amount of OH groups, the adsorption energy for each of the three oxygen intermediates becomes smaller meaning a weaker bond between the Fe–N–C structure and the intermediate. The more labile chemical bonding of oxygen intermediates on more oxidized surfaces may explain the higher catalytic activity and durability of Fe–N–C NH3. While the oxygen adsorption on FeN4 centers remains highly favourable (negative adsorption energies), the oxygen intermediates are more loosely bonded and therefore more likely to evolve further.
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d5cy00124b |
| This journal is © The Royal Society of Chemistry 2025 |