Yuda
Wang‡
a,
Haitao
He‡
a,
Jiao
Sun
*a,
Xinyao
Zhang
a,
Mahmut
Zulpya
a,
Xianhong
Zheng
a,
Lin
Xu
b and
Biao
Dong
b
aDepartment of Cell Biology, College of Basic Medical Science, Jilin University, China. E-mail: jiaosun@jlu.edu.cn
bState Key Laboratory on Integrated Optoelectronics, College of Electronic Science and Engineering, Jilin University, China
First published on 7th July 2023
Ag cluster catalyst-based oxidation of CO to CO2 is an important way to remove CO at low temperatures. However, the instability of silver clusters seriously limits the catalytic application. Herein, sub-nanosized EMT zeolite nanoparticles served as Ag cluster carriers with high selectivity, low coordination, and unsaturated atom active sites. The silver clusters with sub-nanometer size can be controlled with different charge states and loading rates. A detection film with 500 nm was further prepared by assembling the Ag-EMT composites with a small amount of Nalco as an adhesive. For CO detection, a completely enclosed gas sensing device based on in situ infrared spectroscopy was employed without air interference. CO was accurately introduced into the detection chamber and catalysed into CO2 by silver loaded EMT zeolite films, and the whole process was accurately recorded by infrared spectroscopy. CO with a detection range of 2–50 ppm was realized, showing great application potential in gas monitoring.
Zeolites are perfectly suited to accommodate oligoatomic metal clusters due to their molecularly sized cages and channels, and silver nanoparticles (NPs) can normally be embedded with ship-in-a-bottle confinement strategies.32–34 In addition, besides the matrix function, the versatile microporous molecular sieves and especially zeolite with respect to pore structure, surface area, catalytic activity, particle dimensions, and morphology are of particular interest for chemical sensor and membrane applications.
In the case of catalytic oxidation and chemical sensors toward CO at room temperature (RT), a number of investigations on interactions of silver zeolites with carbon monoxide have also appeared in the literature since 1990s. G. Caizaferri et al.35 found the fast and stable co-ordination of CO on Ag+-A zeolite together with the potential to oxidize CO to CO2 completely by adding an optimized amount of water, which could be used for the purification of gases. Water plays a key function in this process. It was also found that Ag+ on Ag-NaY catalyst was very important for the enhancement of CO oxygen activity at low temperatures in the range of 55–70 °C,36 while the exact oxidation process is still a matter of debate. A detailed understanding of this involved process is significant since such small and stabilized Ag clusters, especially when confined in zeolite hosts with excellent stability, having interesting, but so far not well understood, catalytic property.
The motivation for the present work rests on the controlled synthesis of silver cluster loaded nanosized EMT zeolites with different charge states and loading amounts and further assembly in thin films for the detection of carbon monoxide at room temperature (RT). In the preparation process, a small amount of Nalco was employed as a binder, which also can provide the hydroxy groups and play a similar role as water in G. Caizaferri's work.35 Based on the catalytic oxidation property of the Ag-loaded EMT zeolite films, the low concentrations of CO can be detected by monitoring the amount of CO2 by in situ IR spectroscopy.
The EMT zeolite formed stable colloidal suspensions and the silver ion exchange was performed in an aqueous medium to avoid agglomeration. The ion-exchange process was performed as follows: 20 ml silver perchlorate solutions with a concentration of 0.05 M were added to three dispersed EMT zeolite suspensions (7.5 wt%, 12 ml) and kept for 2 h and 6 h. The ion-exchanged samples were purified three times via high-speed centrifugation and redispersed in water. The reduction of silver cations to nanoparticles (Ag NPs) in the EMT zeolite suspensions (2 wt%, 7 ml) was obtained under microwave reduction (120 °C, 10 min, 1000 W, Anton Paar Synthos 3000) in the presence of triethylamine as reducing agent (N(C2H5)3, 0.5 ml, 2 ml, and 4 ml). The reduced suspensions were again purified three times and finally dispersed in water. For clarity, the samples with different ion exchange times can be divided as Ag+-EMT-1 (ion exchange time: 2 h) and Ag+-EMT-2 (ion exchange time: 6 h). After reduction with an increasing amount of reducing agent (N(C2H5)3, 0.5 ml, 2 ml, and 4 ml), the samples can be abbreviated as Ag-EMT-1a (0.5 ml N(C2H5)3), Ag-EMT-1b (2 ml N(C2H5)3), Ag-EMT-1c (4 ml N(C2H5)3), Ag-EMT-2a (0.5 ml N(C2H5)3), Ag-EMT-2b (2 ml N(C2H5)3), and Ag-EMT-2c (4 ml N(C2H5)3).
The silicon wafers (100) were precleaned with ethanol and acetone prior deposition of the films. To ensure the preparation of smooth and homogeneous films, the Ag-EMT coating suspensions were filtrated through syringe filters (450 nm), and the spin coating procedure (acceleration: 5000 rpm s−1, 5000 rpm for 180 s) was repeated 5 times (each coating step uses three drops of suspension, after which the films were dried at 90 °C for 30 min). The final films have a thickness of 500 nm and cover entirely the silicon wafers with a dimension of 10 × 10 mm2.
Fig. 1 (a) The experimental setup for CO sensing with a gas flow system and in situ IR reactor cell. (b) Scheme of the in situ IR system for detection of CO with Ag-containing zeolite films. |
The two gases (mixed gas of Ar and CO and pure Ar) were sent independently to the IR reactor cell. The gas compositions used for the experiments are as follows: activation flow, Ar with a total flow of 25 cm3 min−1; reaction flow, CO with a concentration of 2–50 ppm, diluted in Ar with a total flow of 20 cm3 min−1. The ZnO/SnSe2 sensor developed by Wang et al.4,5 had the maximum response in the CO concentration range of 10–1000 ppm, with a maximum response of 200 ppm CO. In situ IR molecular detections of a single gas or mixtures were carried out at 25 °C. The IR spectra were collected in a continuous mode (64 scans per spectrum) with a Tensor37 spectrometer (Bruker) equipped with a DTGS detector.
The different amounts of loaded silver can also be proved by the TG measurements. The weight loss curve of TG results before 250 °C corresponds to the water inside the supercages, which stabilizes the silver ions. It can be seen that the water content of pure EMT and silver containing EMT samples also decrease with the increase in silver amount (Fig. 2c).
Sub-nanometer sized silver clusters in Ag-EMT zeolite can be recorded by TEM measurement on the cupper grid. From the enlarged images of the sample, extremely small spots having a higher contrast than the zeolite, possibly related to the presence of confined silver clusters, are exclusively detected inside the sodalite cages of the EMT nanocrystals (Fig. 2d). To investigate the position of the silver clusters, the schematic diagram of EMT framework structure was overlapped with the TEM images, and the results show a good match and the silver clusters (black dots) stay separately in the sodalite cages.
The XPS results of the synthesized nanozeolite are shown in Table 1. From the surface analysis, the Si/Al, Ag/Al, and Na/Al ratios are similar between the reduced and unreduced samples. It means the microwave reduction did not cause the silver loss in the crystal growth process.
Sample | Si/Al | Ag/Al | Na/Al |
---|---|---|---|
Ag+-EMT-1 | 1.24 | 0.22 | 0.56 |
Ag0-EMT-1b | 1.25 | 0.24 | 0.62 |
Ag+-EMT-2 | 1.25 | 0.63 | 0.24 |
Ag0-EMT-2b | 1.16 | 0.64 | 0.21 |
The particle size and stability of the Ag-containing nanosized crystals in the coating suspensions prior to film deposition are studied by DLS. The sizes of the Ag-EMT nanoparticles (NPs) with different silver concentrations were measured to be about 50 ± 5 nm, as shown in Fig. 3a and b. The result is slightly bigger than that determined with TEM, which could be explained by the dynamic interactions between the zeolite nanoparticles, their surface structure, concentration, and ions present in the dispersion medium. The ζ potential value using the Huckel equation for all the samples is about −40 mV, which corresponds to stable colloidal suspensions. Irreversible agglomeration of the crystalline Ag-EMT nanoparticles in the suspensions was not observed for a period of 24 months; i.e., no change of ζ potential value was found for this period. The previously reported pd-modified WSe2 (Pd–WSe2) nanosheet sensors and ZnO/SnSe2 composite film sensors developed by Wang et al.4,5 were exposed to different concentrations of CO gas with no significant change in the percentage response over 30 days, which also confirms its good long-term stability. Though naked silver clusters are not stable in the solution, they can be well protected with the zeolite channels. To further prove the great colloidal stability of Ag-EMT NPs, the colloidal solution (before and after reduction) was placed in an oven, and then the zeolites became aligned wires during the water evaporation process, indicating that the zeolite nanocrystals have always been in a colloidal state and slowly aligned as wires with evaporation (Fig. S1†).
The stable Ag-EMT suspensions were spin-coated on thin films on the silicon wafers. The samples have the same thickness since they pass the same spin-coating procedure. Side and top views of Ag0-EMT-1b (Fig. 3c) and Ag0-EMT-2b (Fig. 3d) by SEM and AFM measurements are selected as examples. The zeolite crystals are well-packed and form dense and homogeneous films with an ultimate thickness of about 500 nm. The surface feature from AFM measurements confirms the flat morphology of the films. The size of the embedded particles is estimated to be 20–30 nm, in good agreement with TEM measurements.
The spectra for the detection of CO on Ag0-EMT-2b film are shown in (Fig. 4a). As can be seen, adding CO to the Ag-EMT sample leads instantaneously to the appearance of a gas phase CO2 band centered at 2236 and 2210 cm−1. Meanwhile, the characteristic bands of adsorbed carbon monoxide on the Ag and Al cations in zeolite appear from 2200 to 2275 cm−1. Increasing the CO concentration from 2 to 50 ppm at room temperature (RT) resulted in an increased intensity of CO2. The intensities of CO2 dependent on the amount of CO were plotted (Fig. 4b). As can be seen, the intensity of the CO2 band increases in both silver containing films, but no CO2 signal was observed for the pure EMT films. In Ag0-EMT-2b film, a liner trend dependent on the CO concentration can be found before 35 ppm and then the saturation is reached. However, for Ag-EMT-1b film, no saturation appears in the range of 2–50 ppm, but the intensity is lower than that with a higher amount of silver. In the case of CO sensing, it is very important for the detection in this range since human health can be harmed by CO with more than 30 ppm.37
Considering that the optical path in the IR machine was filled with nitrogen, the detected CO2 should be in the cell and comes from the transformation of oxidized CO. Note that the size of the individual zeolite nanocrystals and the thickness of the films are comparable, while the silver contents in samples are 0 wt%, 9 wt%, and 18 wt% from ICP analysis, respectively, which is also in good accordance with the changes of the CO2 intensity. Therefore, the silver inside the zeolite plays a key role in the catalytic oxidation of CO.
Since there is no oxygen gas in the system, some oxygen species should exist in the film. Normally, water can be involved in the oxidation of CO to CO2 from the results of G. Caizaferri et al.35 In this work, we suppose that the binder Nalco plays a similar role to water since it has much more hydroxyl groups besides the function of crosslinker. It is also confirmed by the same experiment with the film of Ag–zeolite without Nalco binder, which shows no CO2 signal (Fig. S2†). Considering the reaction in the results of G. Caizaferri et al.,35 we propose a possible reaction with the following equation: 6Si–OH + CO + 2Ag+ → 2Ag0 + CO2 + 3Si–O–Si + 2H3+O, which is catalyzed by silver clusters in the zeolite. [EMT]-Ag+-[CO(OH)]− radical can be supposed as a hypothetical intermediate in the reaction.33
To elucidate further on this point, the CO2 intensities dependent on CO with Ag+-EMT and Ag-EMT samples were carried out, as shown in (Fig. 5a and b). In both cases, only weak bands of CO2 were found in high concentrations of CO for unreduced Ag+-EMT samples. As the reducing agent increases, more and more silver cations are reduced to silver NPs, while the CO2 intensity dependent on CO shows an opposite trend in both cases. Among Ag-EMT-2a, 2b, and 2c samples (Fig. 5c and d), the CO2 intensity increases with the increase of the silver metal amount, which indicates that more silver metal promoted the catalytic oxidation of CO. While in the sample of Ag-EMT 1a, 1b and 1c, increasing the reducing agent causes a much slower reaction. Considering the above supposed reaction, these results further confirm that both silver cations and silver NPs are involved in the catalytic oxidation, and serve as reactant and catalyst, respectively. The total amount of silver in EMT zeolite is certain after the ion exchange. Therefore, in Ag-EMT 1a, b, c samples, the reaction speed depends very much on the amount of silver cations, which will be less and less in the reducing environment. While in the sample Ag-EMT 2a, b, c, there are enough silver cations in the EMT zeolite due to the long-time ion exchange even with high amounts of reducing agent. Therefore, more amount of silver metal can serve as a catalyst and control the oxidation behavior.
Comparing the two Ag+-EMT samples, both of them show no reaction activity as the CO concentration is low. As the CO amount increases, Ag+-EMT-2 shows a little more reactivity relative to Ag+-EMT-1, while it is still much lower relative to the reduced samples. On the other hand, the weak signal from Ag+-EMT-1 and Ag+-EMT-2 can also suggest that a small amount of silver NPs existed inside the zeolites, which should have formed in the film preparation (spin-coating) process since evaporation of the solvent can also cause the reduction of a small amount of silver. The phenomenon of evaporation of Ag-EMT suspensions in glass bottles can further prove this, as shown in (Fig. S2†). The above results indicate that the condition for the reaction is that Ag cations and Ag NPs are available simultaneously.
The Ag NPs with the sub-nanometer size or clusters are saturated in the sodalite cages, which is proved by the TEM measurements. The hard template effect of zeolite makes the Ag NPs very stable as well as accessible due to the molecular sieve property. Though CO cannot enter the sodalite cage because of its size, catalytic oxidation still happens inside the zeolite in the presence of OH groups and silver cations.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3na00238a |
‡ Yuda Wang and Haitao He contributed equally to this work. |