Black metal oxides with varying concentrations of O-vacancies display enhanced optical and catalytic properties. However, direct solution syntheses of this class of materials have been limited despite being highly advantageous given the different synthetic handles that can be leveraged towards control of the targeted material. Herein, we present an alternate colloidal synthesis of black In2O3−x nanoparticles from the simple reaction between In(acac)3 and oleyl alcohol. Growth studies by PXRD, TEM, and STEM-EDS coupled to mechanistic insights from 1H, 13C NMR revealed the particles form via two paths, one of which involves In0. We also show that variations in the synthesis atmosphere, ligand environment, and indium precursor can inhibit formation of the black In2O3−x. The optical spectrum for the black nanoparticles displayed a significant redshift when compared to pristine In2O3, consistent with the presence of O-vacancies. Raman spectra and surface analysis also supported the presence of surface oxygen vacancies in the as-synthesized black In2O3−x.
Oxygen vacant metal oxides have a non-stoichiometric oxygen composition. The non-stoichiometry or oxygen deficiency can arise from “self-doping”. This effect is a result of aliovalent constituent metal species, resulting in the elimination of oxygen as a means of maintaining charge neutrality.16–22 Additionally, the elimination of oxygen results in discrete regions of disorder (amorphization) in the lattice.16,21,23 While oxygen vacancies and their effects have been known for some time, one of the most notable reports on the topic came from Chen and co-workers in 2011 through the controlled hydrogenation of TiO2 nanoparticles.24 The hydrogenated particles shifted from white to black exhibiting an extreme extension of absorbance into NIR region. This resulted in a paradigm shift in the way researchers approached the development of visible light absorbing photo(electro)catalysts.
In addition to TiO2, metal oxides such as In2O3, CeO2, ZrO2 and WO3 have all displayed an extended absorption range, as well as other distinct properties through oxygen vacancy control.14,16,25–27 Ozin and co-workers evaluated black In2O3 under photothermal conditions which displayed a relative fivefold increase in the production of CO from CO2 hydrogenation under illuminated and varying temperature conditions when compared with pristine In2O3.16,28 Tungsten oxides, having a slew of sub-stoichiometric compositions (WO2.72, WO2.8, WO2.83, and WO2.9) display surface plasmon resonance (SPR) extending absorbance into the NIR. Additionally, Xie and co-workers reported extended catalytic activity in reduced WO3 through the continued degradation of formaldehyde which continued 5 h post-illumination.27,29,30
The formation of oxygen vacancies has been predominately achieved though post-synthetic methods including, plasma treatment, laser irradiation, and electrochemically.31–33 However, the most common method has been via hydrogenation.3,4,16,18,20,34–36 While effective, this approach requires high temperatures (i.e., energy demand) and a hydrogen atmosphere which albeit not uncommon can present safety concerns. The elevated temperatures can also lead to sintering which decreases the surface area, an important property for catalytic applications.37
Solution based synthesis offers an alternative to these harsh conditions but only a few have been reported. Fang and co-workers produced black TiO2 post-synthesis via the generation of in situ H2 from the addition of sodium borohydride to an aqueous particle suspension.25 Similar results were reported by Jung and co-workers following an analogous approach that used 2-methylimidazole under aqueous conditions as well.38 Alternatively, the direct synthesis of materials with oxygen vacancies using precursor chemistry offers a more facile approach, eliminating the need for particle formation followed by post-treatment. Several methods have been reported to prepare WO3−x using precursors with readily oxidizable W4+ or W5+.27,29,39 Guo and co-workers developed a solvothermal method based on cerium(III) acetylacetonate which resulted in reduced CeO2 quantum dots at temperatures as low as 120 °C.20 Recently, Milliron and co-workers reported a colloidal synthesis to produce oxygen deficient In2O3 through the presence of spectator cations which was extended to CdO and γ-Fe3O4.26
Herein, we report on an alternate non-aqueous colloidal synthesis of black, oxygen deficient In2O3−x nanoparticles. The synthesis is based on the reaction between indium(III) acetylacetonate (acac) and oleyl alcohol. Control experiments and in-depth analysis of the reaction using NMR revealed the importance of the synthesis atmosphere, the ligand environment, and the acac precursor in the formation of In2O3−x. PXRD and STEM-EDS elemental mapping provided unique insight into the growth mechanism. Comparing optical and vibrational studies to previous literature reports we find good agreement with the presence of oxygen vacancies. XPS analysis and gas adsorption measurements further validate and provided quantification of the surface vacancies. These findings highlight the importance of understanding reaction mechanics and nanoparticle growth, to be used to develop broadly absorbing photoactive materials through highly versatile colloidal means.
In a typical synthesis of 9 nm In2O3 nanoparticles, a precursor solution of 1.0 mmol of In(acac)3 was dissolved in 2.0 mL of OLAC in a 20 mL scintillation vial. The vial was placed on a hot plate in an Al foil jacket with stirring set to 700 rpm and was degassed for 30 min at 120 °C. The vial was then placed under N2 blanket and heated to 150 °C for 30 min. Concurrently, 10.0 mL of OLOH were degassed for 1 h at 120 °C in N2 flow configuration with stirring set to 700 rpm. The reaction was then switched to nitrogen flow and heated to 290 °C. The precursor solution was then loaded into a 5 mL syringe and injected via syringe pump at a rate of 3.5 mL min−1. Upon completion of the injection the reaction was aged for 5 min. The heating mantle was removed, and the flask was cooled naturally to room temperature. The particles were washed three times by precipitating with ethanol and acetone (50/50 vol.), centrifugation at 10000 rpm for 2 min, and resuspension in hexanes. The washed particles were stored in 10.0 mL of hexane.
In efforts to improve the morphology (size/shape) we began by varying reaction conditions starting with the solvent volume. During these studies we observed that decreasing the volume of the reaction from 25 mL to 12 mL enabled more mild reactions conditions with a more abrupt appearance of the black color at ∼210 °C and the reaction temperature lowered from 320 °C to 270 °C. While the crystal domains seemed to decrease in size as evident by a slight widening of the PXRD reflections, particles remained heavily agglomerated (Fig. S3†). We then explored the addition of different ligands. Introducing DOA or TOA had a slight improvement in shape and resulted in smaller agglomerations. Conversely, addition of OLAM or OLAC yielded small, off-white nanoparticles (Fig. S4 and S5†). The production of white nanoparticles when using OLAM and OLAC was surprising and will be discussed below. Due to the improvement of morphology when employing the more substituted amines, we opted to utilize DOA in our finalized procedure.
We then focused our efforts on interrogating early stages of the reaction to gain insights on the growth process of the black In2O3−x. A series of aliquots taken at different time intervals during the reaction were analyzed using PXRD, TEM and STEM-EDS imaging/elemental mapping. For simplicity, Fig. 2 contains data related to the first aliquot and the final product. At time 0 min, defined as the onset of black coloration around 210 °C, the PXRD pattern revealed the unexpected presence of In2O3 and indium metal. TEM imaging, seen in Fig. S6,† showed two distinct particle populations with lattice fringes corresponding to highly polycrystalline In2O3−x and large In particles, in agreement with the PXRD including the relative broadness of the reflections (e.g., In (101) vs. In2O3 (222)).
STEM-EDS elemental mapping (Fig. 2) validated these observations and further showed the presence of an oxide shell on the In particles. Analysis of the aliquots taken as the reaction reached the final temperature (270 °C) showed improved crystallinity of the In2O3−x and a gradual decrease of the reflections corresponding to In (Fig. S7†). After 1 h at 270 °C, the observed diffraction pattern is predominately that of In2O3 with perhaps a minor contribution of In, convoluted by overlapping of the In2O3 (312) and In (101) reflections (Fig. 2). STEM-EDS elemental mapping revealed the In particles convert to In2O3−x with some containing an In rich core as seen in Fig. 2. Line-scans of the In rich core shows these are not pure metal but rather highly O-deficient regions (Fig. S8†). It should be noted that we did not observe any hollow structures, indicating the Kirkendall effect was not at play. Taken together, the results from the aliquot study suggest a poorly oxidative reaction environment, favoring the reduction of the In(acac)3 precursor to In0 and oxygen deficient In2O3−x. A poorly oxidative reaction environment was also recently reported by Robinson et al. in the synthesis of CoMn2O4 spinels.45
To complement the TEM aliquot studies, we performed Rietveld refinement on the onset and final reaction samples. This method provides the relative percentages of a mixture and stoichiometric information. Fig. S9† shows the refined patterns with tabulated results seen in Table S1.† Analysis of the onset pattern reveals the relative percentage of In metal is ∼37%, which decreases to ∼4% in the final particles. By refining the oxygen occupancy in the onset and final samples, both display an oxygen deficiency of approximately 10% supporting the hypothesis that the oxide is oxygen deficient from an early stage. As control, we performed the same analysis for 120 nm pristine In2O3 control sample (vide infra) which showed no presence of In metal and a stoichiometric composition, validating our refinement model.
In order to probe the reaction environment, we performed the synthesis under altered conditions. First, the synthesis was done under ambient atmosphere by leaving the condenser open. The reaction proceeded similarly with formation of the black In2O3−x product (Fig. S10†). In contrast, syntheses carried out saturating the flask headspace with air flow or bubbling air directly into the solution yielded off-white, pristine In2O3 (Fig. S10†). As expected, the increased supply of air creates a more oxidizing environment that prevents the reduction of In3+ and inhibits the formation of the black oxide, while the open condenser setup most likely does not allow for a significant mixing of the ambient air during the reaction. It should be noted that exposure to air during the synthesis can be used to provide some tunability of the stoichiometry (vide infra), albeit not full control. Aside from the reaction atmosphere, other factors that play a role in the formation of the black In2O3−x were the ligand environment and the metal precursor. As mentioned earlier, addition of OLAM or OLAC to the reaction under a N2 atmosphere yielded off-white, pristine In2O3 nanoparticles (Fig. S5 and S4†). When In(acac)3 is replaced with In(OAc)3 under otherwise identical conditions (DOA, OLOH, N2 atmosphere at 270 °C) the obtained product was also pristine In2O3 as seen in Fig. S5.†
To gain a more mechanistic understanding of the different reaction outcomes we proceeded to analyze the supernatant of a simplified synthesis that yielded black In2O3−x. Here, 2.0 mL of OLOH were combined with 1.0 mmol of precursor and aliquots were taken at different times and temperatures. This volume was selected as it was the smallest working volume that allowed for 1.0 mmol of precursor to dissolve and react while preventing the potential for signal saturation from unreacted OLOH. The initial focus was the formation of the indium metal.
Given the poorly oxidative reaction environment (demonstrated by the control experiments) the formation of indium metal nanoparticles can be expected, as alcohols are known reducing agents.46–49 However, we wondered whether the alcohol was the active reducing agent or if it first formed an aldehyde. Fig. 3 shows the 1H NMR comparisons of stock OLOH, the degassed reaction supernatant (120 °C, 30 min), the supernatant early in the black color appearance (235 °C), and the full reaction (270 °C, 60 min) (13C NMR spectra Fig. S11†). Observing the region between 9–10 ppm in the 1H NMR spectrum of the full reaction a very small triplet of doublets appears at 9.75 ppm. Due to the very low intensity we failed to see any coupling in the 2D techniques, however when comparing the shift to the spectrum of dodecyl aldehyde (Fig. S12†), the observed triplet is consistent with the analog. Additionally, the splitting is consistent with protons split by alkyl free rotation (∼8 Hz) then split to a smaller extent by the aldehyde rotation (∼2 Hz). It should be noted that the aldehyde triplet appears in the stock OLOH prior to any use, with minimal change in intensity after heating the degassed OLOH alone under the reaction conditions (Fig. S13†). Conversely, an increase in peak intensity was observed in the supernatant of the final reaction spectrum, indicating oxidation of the alcohol as it reduces the indium precursor.
It should be noted that the amount of aldehyde observed in the final product is very minor compared to the relative amount of metal observed throughout the reaction. We would expect the possibility of the aldehyde also serving as reducing agent, further oxidizing to the carboxylic acid. However, we fail to see any of the features associated with such a species. The work done by Lee and co-workers presents one possible explanation for the low concentration of aldehyde. Their work showed the catalytic reduction of an aldehyde to an alcohol with In(iOPr)3 as catalyst following a Meerwin–Pondorf–Verley type mechanism.50 At the elevated temperatures in our procedure, it is very possible an equilibrium exists between the acac and alcohol to form acetylacetone and an oleyl alkoxide. From this we speculated that the aldehyde in our reaction was being catalytically converted back to OLOH. To test this hypothesis, we carried out a 2 mL volume reaction spiked with 1.0 mmol of dodecanal. Comparing the 1H NMR of the mix of OLOH and aldehyde to the supernatant of a completed reaction we observed a drastic decrease in the aldehyde proton signal in the final product (Fig. S14†). We failed to observe any evidence of a carboxylic acid forming suggesting the low amount of aldehyde in the final aliquot does not reflect the true amount generated due to a complex underlying process. Based on these results we propose reaction path 1 illustrated in Scheme 1. At the onset of nucleation/observance of the black color, part of the precursor is rapidly reduced from In3+ to In0 through oxidation of OLOH to oleyl aldehyde and possible conversion of the aldehyde back to the alcohol. With a better understanding of the molecular path that yields the In0 particles, we turned to the oxide formation.
From the comparison of the 1H NMR spectra shown in Fig. 3, we can see distinct changes throughout the progression of the reaction between 1.00–4.25 ppm. The most notable change is the appearance of an additional triplet centered at 4.05 ppm, downfield of a triplet associated with the alcohol 1a protons (Fig. 3a). From its chemical shift in the 13C NMR, the appearance of a new carbon signal at 171.21 ppm, we identified this feature as an ester (Fig. S11†). The intense singlet at 2.04 ppm is coupled to a carbon at 20.95 ppm in the heteronuclear single quantum coherence (HSQC) spectrum (Fig. S15†), both of which display the appropriate chemical shift for an acetate ester with the appropriate phasing displaying CH or CH3 characteristic. The heteronuclear multiple bond correlation (HMBC) spectrum (Fig. S16†) displays coupling to the ester carbonyl, allowing us to assign this as a terminal methyl group adjacent to the ester carbonyl. Presence of an ester was validated by FTIR (Fig. S17†) through the appearance of peaks at 1743 cm−1 and 1237 cm−1 which can be assigned to the ester's CO and C–O stretches, respectively; the latter distinguishable from the alcohol C–O stretch observed at 1051 cm−1.
The other notable feature in the full reaction 1H NMR is the appearance of a small singlet at 2.16 ppm. This signal couples to a small feature in the 13C NMR at 30.84 ppm seen in the 1H NMR and HSQC spectra with CH/CH3 phasing (Fig. 3 and S15†). The appearance of the expected ketone chemical shift in the 13C NMR is not observed, most likely due to a lower concentration of acetone combined with the low sensitivities of carbonyl groups in 13C NMR.51 However, in the HMBC spectrum the singlet at 2.16 ppm displays coupling to a carbon at ∼207 ppm (Fig. S16†). These shifts are consistent with acetone in CDCl3.52
The appearance of an ester and acetone are two of the expected products seen in the literature for the reaction between a metal acac and a primary alcohol.46,48,53 Based on these observations and the lack of features indicative of an ether, the oxide formation mechanism most likely follows the path reported by Niederberger and co-workers as laid out in path 2 of Scheme 1. The alcohol performs a nucleophilic attack on the acac carbonyl while an enolate and ester ligand coordinate to the In center. The ester is released and replaced with water. The water then undergoes proton transfer with the enolate generating acetone and a hydroxyl ligand. The L2In-OH species can then condense to form the oxygen deficient In2O3−x (Scheme 1). When DOA is present, it can also coordinate to the In center. With this mechanism in mind, we provide possible explanations for the different results observed when OLAM, OLAC, or In(OAc)3 were used in the reaction.
The addition of OLAM producing pristine particles and no indium metal (although its role as reducing agent is well documented), suggests it follows a much faster amidation analogue of path 2.45,48,54 Hutchison and co-workers assessed the use of primary amine vs. primary alcohol in the preparation of In2O3 and found that primary amines reacted much faster than the alcohol.54 To validate this report, we performed the same 2 mL volume test by using OLAM instead of OLOH; analyzing aliquots at the same interval with NMR as the OLOH trials seen in Fig. S18.† We tracked the diminishing of the amine adjacent protons at ∼2.66 ppm and the increase of the amide proton signal at ∼3.21 ppm. Forming ratios of amide:amine and ester:alcohol from the integrated proton signals (Table S2†), it can be seen that the amide quantity very quickly over takes the amine by approximate 2.5. In contrast, the ester never overtakes the alcohol amount in the same timeframe, validating the greater reactivity of the amine. To probe the effects of sterics, we replaced the 2 mL of DOA in the reaction with 2 mL of 4-octylaniline. The aniline derivative is a weaker primary amine with sterics between that of OLAM and DOA. The reaction initially turned black at 235 °C which subsequently lightened in color after ∼20 min at 270 °C. The PXRD in Fig. S19† shows a similar pattern to the black oxide pattern with a wider base suggesting increased polydispersity. TEM analysis seen in Fig. S19† shows a mix of large particles similar with the black particles’ morphology and small particles consistent with the pristine ones obtained when using OLAM. This result suggests that aniline initially reacts slow enough to allow for the indium metal and oxygen deficient particles to form but at the final reaction temperature the amidation pathway begins to take over. When OLAC is present in the reaction we posit a similar rate effect as that of the OLAM takes place. The presence of OLAC in the reaction typically results in the in situ formation of a metal oleate that serves as precursor.6,26 The reaction of carboxylates with an alcohol to produce the metal oxide proceeds via a simpler esterification pathway that does not require C–C bond breaking. This simpler pathway would also explain the observed difference in reactivity between In(acac)3 and In(OAc)3 as the acac involves C–C bond breaking while the acetate does not. Performing a similar small volume experiment we added 1 mL (∼3 mmol) of OLAC to the 2 mL of OLOH; a stoichiometric amount relative to the acac ligands. The 1HNMR analysis seen in Fig. S18† reveals an approximate 3 times increase in the ester:alcohol ratio, supporting our hypothesis that a faster condensation reaction occurs between the carboxylate when compared to the acac. Therefore, it is likely a synergistic effect between the acac and primary alcohol which allows for the conditions necessary to form the oxygen vacant oxide.
As illustrated in Scheme 1, the proposed overarching mechanism is as follows. At the visual onset of the black color change the reduction of In3+ to In0 through the oxidation of OLOH to oleyl aldehyde occurs rapidly (path 1) with concurrent formation of oxide particles containing oxygen vacancies (path 2). As the reaction is held at 270 °C for 1 h, the two paths converge (path 3). The metal particles get oxidized to form oxygen deficient In2O3−x with some particles containing an InyOz core while the In2O3−x formed through path 2 becomes more crystalline. The fact that in the standard reaction, all aliquots analyzed were black with their PXRD patterns containing reflections for the oxide is a good indication of oxygen deficient particles. In control reactions where pristine In2O3 particles formed concurrently with In0, the solution color was gray. To further validate that the obtained particles were rich in oxygen vacancies we performed a range of characterization techniques as discussed in the next sections.
Aside from the enhanced optical properties, an additional signature of oxygen vacancies is a significantly altered Raman spectrum. The Millirion group and several other groups have attributed broadened and reduced Raman modes observed in black In2O3−x and other oxygen deficient oxides to phonon confinement.3,26,30,55,56 The phonon confinement arises from oxygen vacancies forming discrete disordered regions as opposed to being randomly distributed throughout the lattice. As a result, the long-range ordering in the lattice is disrupted quenching/broadening many of the expected modes. Such disordered regions have been observed through HR-TEM by the Ozin group and others.16,57,58Fig. 5 displays the Raman spectra for the black In2O3−x and the three control samples (annealed, “9 nm” and “120 nm”). Each control displays defined modes at ∼130, 305, 365, 494, and 627 cm−1, while the black In2O3−x only displays one easily identifiable peak at 127.8 cm−1 with the remaining four modes significantly diminished/broadened or absent. The high degree of crystallinity of the black In2O3−x (as evidenced by PXRD, HR-TEM, and SAED analysis), supports that the less defined spectrum is not due to discrete disordered regions rather than an overall amorphization. Comparing these results with the work of Milliron and coworkers on colloidal black In2O3, we can see a striking similarity between their most oxygen deficient Raman spectrum and our own.26 We also observed a slight red shift in the spectrum for black In2O3−x which has been attributed to laser induced heating of the dark material during measurements.26,55
Fig. 6 XPS spectra of the black In2O3−x, aged black In2O3−x, air annealed, 9 nm pristine, 120 nm pristine, and commercial samples. Each spectrum was fit with lattice and surface hydroxyl groups, while the black In2O3−x samples displayed an additional HBE feature. The Survey scans of each material are found in Fig. S24† and peak fitting parameters for the O 1s fitting are found in Table S3.† |
The O 1s XPS spectrum is commonly reported as tool to characterize and/or quantify oxygen vacancies in metal oxides. The rationale being that the presence of different oxidation states and/or coordination environment in the host metal centers, results in a shift in binding energy of the surrounding oxygen, or the appearance of new peaks. Upon inspection of the O 1s spectra in Fig. 6, a distinct difference is observed in the In2O3−x samples. The shoulder a few eV higher than the strongest peak displays greater broadening and intensity relative to the non-black control samples. By fitting the O 1s spectra of the black and control materials we can relate the areas to approximate atomic % of oxygen species at the surface and up to ∼10 nm within the particles (Fig. 6). From the peak fitting we observed 2 distinct regions corresponding to lattice oxygen of the metal oxide (∼529.5 eV), and surface coordinated hydroxyl groups (∼531.3 eV).64,65 Additionally, we observed a third feature at higher binding energy (∼532.7 eV, further referred to as HBE) of an unknown identity absent in the controls. In other reports, this feature has been assigned to loosely bound water, however this is unlikely under the ultra-high vacuum conditions the measurements are conducted under.
Upon inspection of the spectrum for the black In2O3−x, one can observe a much higher intensity with a larger peak-fit area relating to surface hydroxyl groups. Since the peak area is proportional to concentration, this observation indicates the black In2O3−x contains a higher concentration of surface hydroxyl groups relative to the controls. This result is consistent with literature reports that have shown an increased concentration of surface hydroxyl groups is associated with oxygen deficient metal oxides.28,66 In fact, the majority of oxygen vacant materials display this increase in surface coordinated oxygen containing species.16,26,28,35,66–68 While each of the analyzed materials displayed the expected hydroxyl peak, a comparison of the hydroxyl:lattice (OH:L) ratios (Fig. 6) showed the black In2O3−x displayed almost double the amount of surface hydroxyl groups compared to the control samples. Most notably, the comparison between the black and 9 nm pristine In2O3 eliminates the possibility of a size/surface area component as the larger black In2O3−x far exceed the 9 nm particles in terms of OH:LO ratio; as well as the 9 nm particles experiencing a more complete sampling due to their size. The increase in hydroxyl signal in the XPS fit is consistent with that reported by Milliron and Ozin for black and pristine In2O3.16,26 Furthermore, the appearance of the HBE feature in only the black indium oxide may be a further signature of additional oxygen species quenching the surface vacant sites. The stability of the particles was assessed by XPS analysis of old (>3 months) In2O3−x samples stored in toluene under ambient conditions. The spectrum for this sample (Fig. 6, top right corner) on par with the freshly prepared In2O3−x, indicating a consistent surface environment and long-term stability.
To complement the XPS analysis, we performed gas chemisorption measurement. Rosowski and co-workers utilized a creative approach using constant flow N2O chemisorption to quantify surface vacancies in hydrogenated In2O3 and ZrO2.18 The mechanism of N2O chemisorption has been described as the insertion of oxygen into a surface vacant oxygen site, followed by the release of diatomic nitrogen. As such, it is possible to monitor the consumption of N2O as a means to detect and quantify oxygen vacancies. As discussed above, oxygen vacant sites are higher in energy, making them susceptible to quenching. Prior to the measurements, a mild hydrogen pre-treatment was performed, as reported by Rosowski to strip the nanoparticles of any ligands utilized in the synthesis and surface quenching species.18 Performing the titration following the pre-treatment we observed N2O consumption/evolution in all samples as seen in Fig. S26.† From these measurements, we were able to calculate a surface vacancy density for the 9 nm pristine, 120 nm pristine, and black In2O3−x to be 205.6, 131.3, and 230.8 μmol g−1, respectively. Thus, the black In2O3−x displayed the highest degree of consumption, indicating a higher concentration of vacancies. We acknowledge that the hydrogenation pre-treatment could induce vacancies in all samples. However, from the H2 consumption plots (Fig. S26†) we see a very consistent trend in uptake, suggesting similar responses by each of the trials. Holding all things equal, it would be expected that the higher surface area of the 9 nm pristine In2O3 would have the highest vacancy density, while the 120 nm and black particles would have similar values. Therefore, the larger response of the black In2O3−x can be attributed to the pre-existing vacancies and not from the hydrogenation pre-treatment.
Footnote |
† Electronic supplementary information (ESI) available: SAED, PXRD, NMR, FTIR, XPS, gas adsorption measurements. See DOI: https://doi.org/10.1039/d3nr05035a |
This journal is © The Royal Society of Chemistry 2024 |