Hongbo
Suo
a,
Huining
Geng
a,
Lu
Zhang
a,
Guoyun
liu
a,
Hui
Yan
a,
Rui
Cao
a,
Jiahao
Zhu
a,
Yi
Hu
*b and
Lili
Xu
*a
aSchool of Pharmaceutical Sciences, Liaocheng University, Liaocheng, Shandong 252059, China. E-mail: lilixu66@163.com
bState Key Laboratory of Materials-Oriented Chemical Engineering, School of Pharmaceutical Sciences, Nanjing Tech University, Nanjing 210009, China. E-mail: huyi@njtech.edu.cn
First published on 3rd January 2023
Enzymatic esterification plays an important role in the fields of chemistry and biotechnology. In this study, lipase was immobilized on an ionic liquid (IL)-modified magnetic metal–organic framework (MOF) and used to synthesize isoamyl acetate. The immobilized lipase (PPL-ILs/Fe3O4@MOF) showed 2.1-fold and 1.8-fold higher activity compared to the free and immobilized lipase without ILs (PPL-Fe3O4@MOF), respectively. In addition, the anti-denaturant ability and reusability of the PPL-ILs/Fe3O4@MOF were also higher than those of other samples. The ester yield reached 75.1% when the biocatalyst was used to synthesize isoamyl acetate in hexane. The synthesized supports supplied a good microenvironment for the immobilized lipase through multiple interactions. Results of the structural analysis showed that the conformation state of lipase molecules changed after immobilization. The magnetism of the prepared biocatalyst makes it easy to recycle so that PPL-ILs/Fe3O4@MOF maintained 70.2% of the initial activity after eight cycles. The prepared composite materials exhibited good potential in lipase immobilization with enhanced catalytic ability and stability.
Lipase can catalyze esterification and transesterification reactions, and its application in the synthesis of flavor and fragrance esters is among its important applications.3,4 Enzymatic reactions are promising with high efficiency, specificity and mildness. Studies have shown that short chain esters synthesized by immobilized lipase has good application prospects. Polydopamine and cobalt-functionalized multiwalled carbon nanotubes,5 epoxy-activated cloisite,6 and poly-coated magnetic nanoparticles7 were used to immobilize lipase for the synthesis of short-chain flavor esters. There is a hydrophobic lid-covered lipase active center, which has the characteristics of interface activation.8 Existing research reports have mainly adopted the protein engineering technology to mutate different amino acids in the lid domain of lipase, study the change of lipase properties, or construct a lidless lipase.9,10 By designing appropriate nanomaterials for lipase immobilization, the interaction between materials and lipase can affect the lid domain of lipase, thereby improving the activity, stability, and reusability of lipase.11–13
A reasonable design of the immobilization support and immobilization method can effectively improve the catalytic performance of the enzyme.14 The enzyme is easily affected by environmental factors, such as temperature, pH fluctuation, organic solvents, and small molecule inhibitors. When stimulated by these external factors, the conformation of the enzyme will be disturbed to varying degrees or the structure of the active site of the enzyme will be directly destroyed, resulting in reduced or total loss of catalytic activity. Metal–organic frameworks (MOFs) are extensible network frameworks connected by organic ligands and metal nodes (metal ions or metal clusters). Different nodes and linkers can be assembled to form MOFs with various structures. In addition, the rich functional groups of the framework give them flexible modification characteristics. MOFs have the advantages of ultra-high porosity, adjustable pore size, excellent chemical and thermal stability, and are excellent enzyme immobilization carriers.15–17 The surface of the enzyme has a variety of amino acid residues with rich charge characteristics, which enables interaction with the surface or internal pore chemical components of MOFs, including H-bonding, electrostatic force, van der Waals force, π–π interaction, and covalent interaction. Therefore, it is easy to form a stable enzyme with the complex structure of the MOFs. Furthermore, the ultra-high porosity of MOFs can greatly improve the loading efficiency of the enzyme, and the adjustable pore characteristics are conducive to cutting out the fixed space matching the size of the enzyme. Also, the excellent chemical and thermal stability gives enzymes with the higher stability of MOF composites.18
Furthermore, because of the nanometer size of supports, it's difficult to recover the enzyme–support conjugates from the reaction medium. Researchers have developed many magnetic nanocomposites, such as hydroxyapatite-encapsulated γ-Fe2O3,19 Fe3O4–MCM-41,20 magnetic MOFs,21 Fe3O4/nanotube composites,22 magnetic graphene oxide23 and others24 to enhance the recovery of immobilized enzyme. The well-designed MOF–Fe3O4 composites combined the unique properties of MOFs and magnetism of Fe3O4 into one support. The magnetic separation can greatly improve the reusability of the enzyme.
Improving the microenvironment of immobilized enzyme could be achieved by introducing functional compounds into supports which can enhance the specific action between enzyme and supports. By introducing cross-linking molecules or modifiers between enzyme and supports, the interactions (electrostatic, chemical bond, hydrogen bond, and hydrophilic/hydrophobic interaction) can be improved, such that the active conformation and flexible structure of the enzyme can be effectively protected.25 Ionic liquids (ILs), as green solvents composed of anions and anions, are used in the enzymatic synthesis of chiral alcohols, chiral amines, and sugars and their derivatives, which greatly improve the catalytic effect.26,27 Applying ILs to an immobilized enzyme can also improve the catalytic performance of the enzyme. For instance, we previously used imidazole IL as a crosslinking molecule to prepare a chitosan/SBA-15 composite for the immobilization of porcine pancreatic lipase (SBA-CIL-CS-PPL). We found that the activity of immobilized lipase was 8.3 times that of the free PPL and that 82% activity was retained after repeated use of 10 times.28 Xie and co-workers covalently grafted imidazole-based ILs to magnetic silica composites for lipase immobilization. The immobilized lipase showed good activity when it was used to synthesized trans-free plastic fats. In addition, the prepared biocatalyst didn’t show significant reduction of activity as it was reused several times.29
In this study, IL-modified magnetic MOFs were prepared and used to immobilize lipase for the synthesis of flavor esters. The synthesis process of the composite and the immobilization of lipase are shown in Scheme 1. The type and strength of the force between lipases and supports affect the structure and catalytic performance of the immobilized lipase. Therefore, the novelty of this work focuses on revealing the adaptability between the lipase and supports by studying the surface properties of supports. The conformation of lipase before and after immobilization was investigated using circular dichroism to analyze the mechanism of enhanced catalytic performance. In addition, the composite combines the porosity of MOFs and the magnetism of Fe3O4, which has a high enzyme loading capacity and convenient separation performance. Furthermore, this new biocatalyst has a potential application in the synthesis of other esters. This study prepared a MOF based composite which has good compatibility with biological macromolecules and expanded the method of improving the microenvironment of immobilized enzymes.
Scheme 1 (a) The synthesis route of ionic liquid modified Fe3O4@MOF and (b) schematic illustration of lipase covalent immobilization on ILs/Fe3O4@MOF. |
XRD was conducted to further confirm the formation of Cu-based MOF coated on Fe3O4 nanoparticles and the patterns of supports are shown in Fig. 2a. The characteristic peaks of Fe3O4 for corresponding plane indexes was consistent with the reports.34 For Fe3O4@MOF and ILs/Fe3O4@MOF, the XRD patterns exhibited Fe3O4 characteristic peaks and showed additional peaks, which was consistent with the characteristic peaks of Cu-PABA.32 The results indicate that the successful formation of Cu-based MOF coated on Fe3O4 and the IL grafting did not change the crystal structure of the magnetic MOF nanoparticles.
TGA was conducted under a N2 flow to analyze the thermal properties of supports. The TGA curves are shown in Fig. 2b. As expressed, Fe3O4 showed 3.21% weight loss under 100 °C, which was due to the removal of water. From 100 to 800 °C, Fe3O4 exhibited no weight loss and showed great thermal stability. In the case of Fe3O4@MOF, a weight loss step was seen from 100 to 305 °C due to solvent evaporation from the MOF layer. When temperature ranged from 305 to 445 °C, Fe3O4@MOF showed a 9.26% weight loss which was ascribed to the MOF framework collapse. Compared with Fe3O4@MOF, the weight loss of ILs/Fe3O4@MOF was more severe due to the superposition of the decomposition of ILs and the collapse of the MOF framework. TGA results further proved the successful synthesis of ILs/Fe3O4@MOF.
Magnetic separation can be used to separate the magnetic biocatalyst from the reaction system. The magnetic properties of the composite materials were characterized and the magnetic hysteresis loops are shown in Fig. 2c. We can observe that the coercivity and remanence of all the curves are near zero, which indicates that the supports exhibit superparamagnetism.35 This property facilitated the recovery and reusability of the immobilized lipase. The saturation magnetization (Ms) of Fe3O4@MOF and ILs/Fe3O4@MOF was 51.4 emu g−1 and 36.7 emu g−1, respectively, which is lower than that of Fe3O4 (72.1 emu g−1). The MOF coating and IL introduction decreased the Ms of ILs/Fe3O4@MOF; however, the magnetic response of ILs/Fe3O4@MOF was sufficient for the magnetic separation as seen in the picture located in the lower right corner of Fig. 2c. The use of magnetic separation could reduce the loss of immobilized lipase in the reuse process.
SEM and TEM were conducted to characterize the morphologies and structural properties of Fe3O4@MOF and ILs/Fe3O4@MOF. The images (Fig. 3) revealed that Fe3O4@MOF and ILs/Fe3O4@MOF were spherical nanoparticles. Nanometer size generally has a high specific surface area, which is beneficial to increasing the load of enzymes. The TEM images show that the magnetic MOF nanoparticles were core–shell structures with rough surfaces. Fe3O4 was the core of the magnetic MOF and the outside coating was composed of a Cu-based MOF. Moreover, comparing the TEM images of Fe3O4@MOF and ILs/Fe3O4@MOF, we found that the introduction of ILs did not destroy the core–shell structure. Additionally, the diameters of supports were calculated according to SEM images and the diameter distribution diagram is shown in Fig. S2 (ESI†). The statistical results showed that the average diameter of Fe3O4@MOF and ILs/Fe3O4@MOF was 257 nm and 229 nm, respectively. The addition of ILs in supports may enhance the repulsive force of particles which reduced aggregation of the particles. Therefore, we found that ILs/Fe3O4@MOF has a lower average diameter which implies better dispersibility.
Fig. 3 SEM images of (a) Fe3O4@MOF and (d) ILs/Fe3O4@MOF. TEM images of (b and c) Fe3O4@MOF and (e and f) ILs/Fe3O4@MOF. |
In the lipase structure, a lid composed of polypeptides isolated the active center from substrates. When lipase was placed at a hydrophobic interface, interface activation occurred which opens the lid and made the active center accessible.36 Herein, we use the water contact angle (WCA) to assess the hydrophobicity of supports and the WCA images of samples are shown in Fig. 4. The WCA of Fe3O4@MOF was 45.9°, and the WCA increased to 53.7° for ILs/Fe3O4@MOF. The increased WCA implied the hydrophobicity of ILs/Fe3O4@MOF was enhanced. When lipase is immobilized on ILs/Fe3O4@MOF, the interfacial activation may exhibit more effect on lipase which moved the lid open. The open conformation of lipase may lead to higher activity and the catalytic performance assessment supported the result.
Support | Loading capacity | Immobilization yields | Specific activity |
---|---|---|---|
(mg g−1) | (%) | (U g−1) | |
a The activity of free PPL was 462 U g−1 at pH = 7.0. | |||
PPL-Fe3O4@MOF | 104.7 | 63.2 | 534.8 |
PPL-ILs/Fe3O4@MOF | 113.6 | 71.9 | 968.4 |
Biocatalyst | α-Helix (%) | β-Sheet (%) | β-Turn (%) | Random coil (%) |
---|---|---|---|---|
Free PPL | 25.2 | 22.7 | 19.5 | 32.2 |
PPL-Fe3O4@MOF | 16.7 | 26.4 | 21.2 | 35.4 |
PPL-ILs/Fe3O4@MOF | 15.3 | 28.5 | 21.5 | 34.6 |
We could see that from Fig. 5b, the optimum reaction temperature for PPL-ILs/Fe3O4@MOF and PPL-Fe3O4@MOF was 45 °C, while that for free PPL was 40 °C. When the temperature rose to 60 °C, residual activities for free PPL rapidly reduced to 52.6%, while the value for PPL-ILs/Fe3O4@MOF and PPL-Fe3O4@MOF was 82.3% and 73.1%, respectively. The results indicate that lipase was more stable at a higher temperature after being immobilized. This may be because the interaction between lipase and supports firmly anchored the structure of enzymes, which protected the integrity of lipase.
The stability of immobilized lipase plays an important role in its application. In this work, urea was used to test the tolerance of immobilized lipase to denaturant. As shown in Fig. 5c, the relative activity decreased when the urea concentration increased. When urea concentration rose to 6 M, residual activity for PPL-Fe3O4@MOF, PPL-ILs/Fe3O4@MOF and free PPL was 49.6%, 66.2% and 10.2%, respectively. The results indicate that lipase resistance to denaturants was enhanced after immobilized on the prepared supports. In addition, compared with PPL-Fe3O4@MOF, PPL-ILs/Fe3O4@MOF further enhanced the tolerance of lipase to denaturant. The improvement may be due to the interaction between the carrier and urea molecules, which prevented urea from disrupting the structure of lipase.43 On the other hand, the multiple interactions between the enzyme and carrier strengthened the rigidity and integrity of lipase, which was further analyzed in the secondary structure investigation.
Good reusability can save costs for the application of enzymes, while convenient separation performance can increase production efficiency. PPL-Fe3O4@MOF and PPL-Fe3O4@MOF have strong magnetic responsiveness which improved the biocatalyst recovery. The magnetic separation may reduce the loss of biocatalyst and guarantee that the activity was not affected by the separation process. As seen in Fig. 5d, PPL-ILs/Fe3O4@MOF and PPL-Fe3O4@MOF maintained 70.2% and 63.4% of the initial activity after eight cycles, respectively. The results indicated that the magnetic MOF nanoparticles have good mechanical strength and that the carrier provided an excellent microenvironment for the immobilized lipase. The introduction of ILs can prevent organic solvent molecules and ions in solution from denaturing the lipase through π–π stacking, H-bonding, ion interaction, and coordination bonding.44 The porosity of MOFs is conducive to improving transfer rates of substrates and products, which reduced the inactivation rate of the enzyme.
Fig. 6 Optimization of (a) alcohol/acid molar ratio, (b) reaction temperature, (c) reaction solvents and (d) reaction time for the synthesis of isoamyl acetate. |
As shown in Fig. 6a, the ester yield increased as the molar ratio of alcohol/acid rose to 3:1 from 1:1. This may be because the esterification reaction is reversible and because an appropriate amount of alcohol can promote the formation of esters while excess alcohol can strengthen the mutual collision between substrates.45 However, when the molar ratio of alcohol/acid increases from 3:1 to 5:1, the ester yield decreased because of the high concentration of isoamyl alcohol, which would cause an irreversible denaturation of the enzyme molecules.
We can observe from Fig. 6b that the ester yield increased when reaction temperature ranged in 35–45 °C. This phenomenon may be because, for an endothermic reaction, the increase in temperature can enhance the thermal movement of substrate molecules and promote the synthesis of products. When reaction temperature increased in the range of 45–55 °C, the ester yield decreased. This is because an extremely high temperature will cause lipase denaturation and inactivation, resulting in a decrease in substrate conversion. The ester yield of PPL-ILs/Fe3O4@MOF was 59.6% higher than that of PPL-Fe3O4@MOF (52.7%) at 45 °C. The result demonstrated that the ILs was beneficial to lipase activity because of the H-bonding, π–π stacking, and electronic interaction between ILs and lipase.
Enzymatic esterification usually occurs in organic solvents, which promotes the reaction equilibrium in ester synthesis because of the mutual solubility of solvent and esters. The polarity and hydrophobicity of solvents could intensely affect the catalytic performance of lipase. As observed in Fig. 6c, the reaction showed the highest ester yield in hexane. This may be because hexane has an appropriate hydrophobicity that does not affect the enzyme's micro water layer.6
Lipase catalytic esterification is a time-consuming, multi-step, and complex reaction, and the reaction time effect on the ester yield is shown in Fig. 6d. Under optimized substrate molar ratio, temperature and solvent, the ester yield increased rapidly within the first 12 h and the yield for PPL-ILs/Fe3O4@MOF and PPL-Fe3O4@MOF reached 65.3% and 58.9%, respectively. When the reaction lasted for 24 h, the ester yield for PPL-ILs/Fe3O4@MOF and PPL-Fe3O4@MOF increased to 75.2% and 71.3%, respectively. Lipase should be surrounded by a water layer that maintains the catalytic activity of the enzyme. In the first 12 h, the reaction provided sufficient water for lipase activity to enable the ester yield to increase rapidly. The esterification and hydrolysis reactions gradually reached equilibrium over time, such that the ester yield no longer increases. Considering the relationship between the reaction time and ester yield, we think that the optimum reaction time was 16 h, while the ester yield was 72.3%.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d2tb02246j |
This journal is © The Royal Society of Chemistry 2023 |