M.
Chen†
*a,
M. P.
Nijboer
a,
A. Y.
Kovalgin
b,
A.
Nijmeijer
a,
F.
Roozeboom
a and
M. W. J.
Luiten-Olieman
*a
aInorganic Membranes, Department of Science and Technology and MESA+ Institute for Nanotechnology, University of Twente, PO Box 217, 7500 AE Enschede, The Netherlands. E-mail: m.chen@utwente.nl; m.w.j.luiten@utwente.nl
bIntegrated Devices and Systems, Faculty of Electrical Engineering, Mathematics and Computer Science, MESA+ Institute for Nanotechnology, University of Twente, PO Box 217, 7500 AE Enschede, The Netherlands
First published on 20th June 2023
Atomic layer deposition (ALD) is a widely recognized technique for depositing ultrathin conformal films with excellent thickness control at Ångström or (sub)monolayer level. Atmospheric-pressure ALD is an upcoming ALD process with a potentially lower ownership cost of the reactor. In this review, we provide a comprehensive overview of the recent applications and development of ALD approaches emphasizing those based on operation at atmospheric pressure. Each application determines its own specific reactor design. Spatial ALD (s-ALD) has been recently introduced for the commercial production of large-area 2D displays, the surface passivation and encapsulation of solar cells and organic light-emitting diode (OLED) displays. Atmospheric temporal ALD (t-ALD) has opened up new emerging applications such as high-porosity particle coatings, functionalization of capillary columns for gas chromatography, and membrane modification in water treatment and gas purification. The challenges and opportunities for highly conformal coating on porous substrates by atmospheric ALD have been identified. We discuss in particular the pros and cons of both s-ALD and t-ALD in combination with their reactor designs in relation to the coating of 3D and high-porosity materials.
Besides controlling the film thickness at Ångström or (sub)monolayer level, another primary advantage of ALD is that it allows for conformal coating on high-aspect-ratio topologies and three-dimensionally structured substrates. This makes ALD the technology of choice over alternative deposition techniques, such as chemical vapor deposition (CVD) and physical vapor deposition (PVD), in areas where conformality is critical. In addition to film conformality, ALD can be normally conducted at lower deposition temperatures than CVD due to the different reaction mechanisms involved. Also, novel dedicated (often homoleptic) precursors have been developed with maximum thermal stability to avoid any thermally activated CVD-like reactions on the substrate, yet with increased surface reactivity. This strategy makes the ALD technique suitable for temperature-sensitive substrates, e.g., polymers. A detailed comparison between ALD, CVD and PVD can be found in the reviews by Muñoz-Rojas et al.5,6
Fig. 1 Applications of ALD in the conventional semiconductor industry and other new emerging fields. Adapted from Zhang et al.9 |
At least as importantly, current t-ALD processes suffer from another issue: low deposition rates. Typically, the ALD rates are on the order of 100–300 nm h−1, which is much slower than other vapor-phase deposition methods (CVD, PVD and pulsed laser deposition (PLD)).8 The throughput of ALD is even lower when substrates with high aspect ratio topologies are used. The reason is that it takes more time for pulsing and purging to allow precursors to diffuse into 3D features and reaction by-products to be removed completely.2
• Easier to use (no vacuum)
• Reduced cost of ownership (COO)
• Potential for easier process upscaling to large substrate areas
• Potential for higher throughput (e.g., more wafers per hour)
• More flexible dopant incorporation options by co-injecting more than one precursor and more than one co-reactant at a time.
Fig. 2 Schematic representation of t-ALD and s-ALD. From Muñoz-Rojas et al.5 |
At the same time, significant research efforts have been made to reduce the ownership cost of t-ALD. In this regard, atmospheric-pressure t-ALD has been considered to make it economically viable for some emerging applications (e.g. porous materials).14–16 In the t-ALD reactor, the four sequential steps (pulse-purge-pulse-purge) compose one deposition cycle. Since layer thickness is mainly determined by the number of deposition cycles, shortening the total time needed to complete one cycle will result in increased throughput of the total ALD process. One option here, is to minimize the time needed to reach self-saturation on the substrate surface at any given reaction temperature during pulsing. To achieve this, one possible solution is to increase the flux of these precursors by using higher operation pressures, preferably atmospheric pressure. Given the short reaction time constants (typically < 0.1 s) for most half-reactions in actual film growth, the reduction of precursor and co-reactant pulse times will have a minor effect on the overall deposition rate of a t-ALD process. On the contrary, the times needed to purge out the reactive precursors and by-products by convective flow at a higher pressure can be shortened considerably in combination with a proper reactor design (e.g. small reactor volumes). However, when coating 3D or high-porosity substrates at high pressures, the gas diffusion in deep and narrow pores becomes slower due to Knudsen diffusion (see section 4). Thus a longer gas residence time in the high-porosity substrate is expected. In order to avoid the occurrence of an unwanted CVD reaction regime, longer purging times are needed to prevent the mixture of two reagents. Therefore, the performance of conventional ALD has been compromised with the trade-off between the long purge times to allow for full surface saturation, and minimizing the total cycle time to reach a time-efficient deposition process. By minimizing the necessary precursor gas residence times and the by-product removal times, one will reach the most optimal and cost-effective process.17
In this review, we will focus on the recent developments in ALD processes operated at atmospheric pressure, or even in an open-air environment (numbers of publications and citations on this topic is given in Fig. 3). Previous reviews have been documented on atmospheric-pressure s-ALD from various points of view. For example, Poodt et al.18 provided an overview of different s-ALD reactors designed by various research institutes and companies around the world. Muñoz-Rojas and MacManus-Driscoll11 highlighted the potential of s-ALD in the field of low-cost PV. More recently, Muñoz-Rojas et al.6 compared the different high-throughput ALD approaches from the perspectives of processing time and targeted cost for different industries. This review aims to provide an overview of recent development and applications of both temporal and spatial atmospheric-pressure ALD and their applications in different areas (Fig. 4). The pros and cons of both ALD approaches will be compared. Finally, a future outlook on the development of atmospheric-pressure ALD will be provided.
Fig. 4 Overview of the content structure of this review, illustrating the main sections and their interrelationships (s-ALD = spatial ALD; t-ALD = temporal ALD). |
Fig. 5 (a) Schematic of an open-air close proximity reactor. The ALD coating head shows the gas channels and gas flow. The channels are 0.7 mm wide with a spacing of 1.4 mm. The coating width W is approximately 50 mm. A is the oxidizing reactant, B is the metal precursor, and I is nitrogen. (b) Rotary s-ALD reactor developed by TNO. (c) R2R reactor for flexible substrates developed by Lotus Applied Technology. (d) A simple, atmospheric pressure R2R web coating s-ALD reactor. Reprinted with permission from Poodt et al.,10,18 Levy et al.,22 and Yersak et al.26 |
Afterwards, a new s-ALD reactor concept was developed by TNO in 2010.10 The group designed a rotary lab-scale reactor as schematically shown in Fig. 5b. In the reactor gas injection head, the two half-reaction zones are separated from each other by exhaust zones and gas-bearing planes. The substrate table is rotated by a servo-motor, connected by a drive shaft. The reactor head is mounted on top of the rotary table with the substrate in between, and as a whole, they are placed in a convection oven for heating. This concept was first tested to deposit ∼10 nm thin Al2O3 passivation films in solar cells. The deposition rate of Al2O3 thin films was as high as 1.2 nm s−1 and the layer thickness was homogeneous along the width of the deposition track. This way, the solar cells showed excellent passivation properties after the coating of the layers.10,23 Start-up companies have been successfully founded for the commercialization of both large-scale and pilot-scale equipment, such as Levitech, SoLayTec, and SparkNano in The Netherlands7 and several other companies described herebelow.
One start-up, Lotus Applied Technology developed a roll-to-roll (R2R) reactor for flexible substrates.24 In this configuration, the two precursor zones are separated by an inert gas which also works as a purging zone (Fig. 5c). One of the main advantages of this design is that it can serve for large-area flexible device applications. The first demonstration was the deposition of moisture barrier films of Al2O3 and TiO2 on 100 mm wide polyethyene terephthalate (PET) foils that moved with a speed of over 1 m s−1. Another type of R2R reactor was developed by Maydannik et al.25 In their approach, a rotating drum was used as a support for the flexible web substrate, placed in a heated cylindrical chamber. The web was exposed to various inlet gas and purge zones with one rotation being equivalent to one ALD cycle. It was demonstrated that flexible substrates with a width of 300 × 100 mm2 could be coated uniformly. However, these R2R reactor concepts are operated at a pressure of about 2 mbar, similar to that in conventional ALD. This low pressure was used to guarantee the individual reaction zones.
To take R2R ALD one step further in scaling up at reduced capital cost, Yersak et al.26 developed a simple, atmospheric pressure R2R web coating system in 2014. The configuration of this web coating system is shown in Fig. 5d. A modular ALD gas source head was designed with the first 10 nozzles filled with N2, followed by sets of precursors and N2 bands. The polymer used in the study was polyethylene naphthalate (PEN) with foil length and width dimensions of 4 m × 100 mm. The PEN web was fastened on four rollers with Kapton tape and circulated in a loop using a belt-driven motor system. Sustained by computational fluid dynamics (CFD) modelling, the appropriate deposition parameters could be first identified. In addition, a spectral reflectometer was mounted onto the injection module to measure the layer thickness and uniformity in situ. Al2O3 was then grown at 100 °C at a rate of 0.11–0.13 nm per cycle, with ALD cycle times of 76 ms and a web speed of 1 m s−1. Later, Ali et al.27,28 also designed a similar R2R system working at atmospheric pressure. A movable web of PET was used as the substrate onto which Al2O3 was deposited at 50 °C at a web speed of 7 mm s−1. The deposited films had a low roughness and good chemical, electrical and optical properties.
The use of water as a co-reactant is common in most ALD processes as it is inexpensive and easily available. However, its vapor pressure and high sticking coefficient can also cause issues such as low reaction kinetics and, in particular, the need for longer purging times. In addition, polymer substrates are very sensitive to temperature. Deposition at low temperature (e.g., room temperature) is preferred in this case. To this end, researchers from TNO started incorporating a dedicated low-damage DBD (dielectric barrier discharge) plasma source into the s-ALD reactor at atmospheric pressure in 2011. This way, Al2O3 films could be deposited at 150 °C using trimethyl aluminium (TMA) in combination with such a DBD plasma-enhanced O2 source.29 By switching on and off the plasma at specific locations, 2D deposition patterns were created. Later, the University of Wuppertal in cooperation with the company SENTECH Instruments also demonstrated a home-built atmospheric-pressure s-ALD equipped with a DBD source.30 The authors deposited TiOx at room temperature with a growth rate comparable to the one reported for low-pressure plasma-enhanced ALD (PE-ALD) or sol–gel processing. The minor contribution of CVD to the growth rate was supposed to be caused by the residual water present in the system.
Integrated circuits (IC) are the backbone of micro- and nanoelectronic devices. One driving force to favor the high-throughput s-ALD concept in commercial IC mass production would certainly be the lower cost.7 Jusung Engineering31 was one of the very first companies to introduce low-pressure s-ALD to the semiconductor industry. Using their advanced “Cyclone” s-ALD reactor they realized 3D multiple (MIMIM) capacitor layer stacks of TiN/Al2O3/TiN/Al2O3/TiN deposited on an (arsenic) n++-doped Si-substrate with macropore arrays etched with ∼1.5 μm pore diameter and 30 μm pore depth.32 TiN layers were deposited at 400 °C at 500 mTorr from TiCl4 and NH3 vapor dosing using sub-second pulse-purge exposures. To avoid oxidation of the TiN electrode layers and thus maintaining the conductivity of the electrodes (<200 μΩ cm), the Al2O3 layers were grown in a separate chamber without breaking the vacuum using PE-ALD in O3 from TMA at 380 °C and 1.2 Torr and 1.2 Torr, using TMA/purge/O3/purge exposures of 0.5/2/3/2 seconds. Later, the low-pressure s-ALD market was dominated by Tokyo Electron (TEL) with their NT-333™ semi-batch reactor.33 In subsequent years, similar reactor designs were realized by several other companies such as Applied Materials,34–36 Lotus Applied Technology,37 Beneq Oy,38 Wonik IPS39 and NCD.40Table 1 gives a short overview of s-ALD reactors offered commercially.
Company | s-ALD reactor name |
---|---|
Applied Materials | Olympia™ |
Beneq Oy | Beneq C2R |
Jusung Engineering | Cyclone |
Lotus Applied Technology | Vortex ALD™ |
NCD | Lucida™ S |
Tokyo Electron (TEL) | NT-333™ |
Wonik IPS | HyEta™ |
Fig. 6 Pie chart distributions of atmospheric-pressure ALD studies conducted in 2008–2023 on materials (left) and applications (right). |
Materials | Precursor | Co-reactant | Substrate | Deposition temperature | Applications | ALD type | Year | Ref. |
---|---|---|---|---|---|---|---|---|
AZO = aluminum-doped ZnO; PFE = printed flexible electronics; IZO = in-doped ZnO; TEMAZ = tetrakis(ethylmethylamino)zirconium; IGZO = InGaZnO; TTIP = titanium isopropoxide; ZTB = zirconium tert-butoxide; DMAI = dimethylaluminum isopropoxide; EG = ethylene glycol; CuhfacTMVS = Cu(1,1,1,5,5,5-hexafluoroacetylacetonate)trimethylvinylsilane; Ag(fod)(Pet3) = triethylphosphine (6,6,7,7,8,8,8-heptafluoro-2,2-dimethyl-3,5-octanedionate) silver(I); TAA = bis(tert-amyloxide); MIMC = metal–insulator-metal capacitors; (NHC)Ag(hmds) = 1,3-di-tert-butyl-imidazolin-2-ylidene silver(I) 1,1,1-trimethyl-N-(trimethylsilyl)silanaminide; Cp = cyclopentadienyl; Et = ethyl; Sn(acac)2 = tin(II) acetylacetonate; RT = room temperature; AS-s-ALD = area-selective spatial ALD; PE-s-ALD = plasma-enhanced spatial ALD; BDEAS = bis(diethylamino)silane. | ||||||||
ZnO | DEZ | NH3/H2O/O2 | Glass coated with Cr and Al2O3 film | 250 °C | TFTs | s-ALD | 2008 | 22 |
Al2O3 | TMA | H2O | Silicon | 200 °C | TFTs | s-ALD | 2009 | 45 |
ZnO | DEZ | NH3/H2O/O2 | Glass coated with Cr and Al2O3 film | — | TFTs | s-ALD | 2009 | 45 |
ZnO | DEZ | H2O | Silicon/glass coated with Cr | 100–250 °C | TFTs | s-ALD | 2012 | 46 |
IGZO | TMIn/TEGa/DEZ | H2O | Silicon | 200 °C | TFTs | s-ALD | 2015 | 43 |
IZO | TMIn/DEZ | N2/O2 | Silicon | 160 °C | TFTs | PE-s-ALD | 2018 | 47 |
IGZO | TMIn/TEGa/DEZ | N2/O2 | Glass | 160 °C | TFTs | PE-s-ALD | 2019 | 48 |
SnO2 | Sn(acac)2 | H2O | Glass | 270 °C | TFTs | s-ALD | 2022 | 49 |
Al2O3 | TMA | O3 | Silicon | 100–200 °C | TFTs | PE-s-ALD | 2022 | 50 |
SnO | Sn(TAA)2 | H2O | Silicon | 100–210 °C | TFTs | s-ALD | 2022 | 51 |
ZnO | DEZ | H2O | Glass | 50–200 °C | Optoelectronic | s-ALD | 2022 | 52 |
TiO2 | TiCl4 | H2O | Glass | 150 °C | Optoelectronic | s-ALD | 2022 | 52 |
Al2O3 | TMA | H2O | Glass | 100–200 °C | Optoelectronic | s-ALD | 2022 | 52 |
N-doped ZnO | DEZ | NH3/H2O | Silicon | 100–300 °C | Solar cell | s-ALD | 2008 | 53 |
Al2O3 | TMA | H2O | Silicon | 200 °C | Solar cell | s-ALD | 2010 | 10 |
Al2O3 | TMA | H2O | Silicon | 200 °C | Solar cell | s-ALD | 2011 | 54 |
TiOx | TIP | Ar/O2 | Silicon/glass | RT | Solar cell | PE-s-ALD | 2013 | 30 |
ZnO | DEZ | NH3/H2O | ITO/glass | 150 °C | Solar cell | s-ALD | 2013 | 55 |
TiO2 | TiCl4 | H2O | ITO/glass | 100/350 °C | Solar cell | s-ALD | 2013 | 56 |
ZnOS | DEZ | H2O/H2S | Silicon | 120 | Solar cell | s-ALD | 2015 | 57 |
AZO | DEZ/TMA | H2O | Silicon | 200 °C | Solar cell | s-ALD | 2015 | 57 |
Zn1−xMgxO | DEZ/Mg(CpEt)2 | H2O | Cu2O | — | Solar cell | s-ALD | 2015 | 58 |
ZnOS | DEZ | H2O/H2S | Silicon | 120 °C | Solar cell | s-ALD | 2016 | 59 |
ZnO | DEZ | H2O | ITO/glass | — | Solar cell | s-ALD | 2016 | 60 |
ZnO | DEZ | H2O | Cu2O | 150 °C | Solar cell | s-ALD | 2016 | 61 |
ZnMgO | DEZ/Mg(CpEt)2 | H2O | Cu2O | 150 °C | Solar cell | s-ALD | 2016 | 61 |
ZnO | DEZ | H2O | Glass | 250 °C | Solar cell | s-ALD | 2017 | 62 |
AZO | DEZ/TMA | H2O | Glass | 250 °C | Solar cell | s-ALD | 2017 | 62 |
Al2O3 | TMA | H2O | ZnO nanorod arrays | 100–350 °C | Solar cell | s-ALD | 2017 | 63 |
ZnO | DEZ | H2O | ZnO nanorod arrays | 100–350 °C | Solar cell | s-ALD | 2017 | 63 |
Cu2O | Cupraselect | H2O | ZnO nanorod arrays | 100–350 °C | Solar cell | s-ALD | 2017 | 63 |
N-doped ZnO | DEZ | 30% NH3 in H2O | ZnO nanorod arrays | 100–350 °C | Solar cell | s-ALD | 2017 | 63 |
Zn1−xMgxO | DEZ/Mg(CpEt)2 | H2O | ZnO nanorod arrays | 100–350 °C | Solar cell | s-ALD | 2017 | 63 |
ZnO | DEZ | H2O | Silicon/glass | 95 °C | Solar cell | s-ALD | 2018 | 64 |
ZnOS | DEZ | H2O/H2S | Silicon/polyamide foil | 100–200 °C | Solar cell | s-ALD | 2018 | 65 |
SnOx | TDMASn | H2O | Glass | 80–150 °C | Solar cell | s-ALD | 2018 | 66 |
NiOx | Ni(MeCp)2 | O2 | Glass | 350 °C | Solar cell | s-ALD | 2018 | 67 |
Cu2O | CuhfacTMVS | H2O | Silicon | 200/220 °C | Solar cell | s-ALD | 2021 | 68 |
TiO2 | TTIP | H2O | Glass | 100–300 °C | Solar cell | s-ALD | 2021 | 69 |
TiO2 | TiCl4 | H2O | Glass | 100–300 °C | Solar cell | s-ALD | 2021 | 69 |
Al2O3 | TMA | He/O2 | Silicon | 150 °C | Patterned deposition | PE-s-ALD | 2011 | 29 |
ZnO | DEZ | H2O | Silicon/glass | 100–300 °C | Patterned deposition | AS-s-ALD | 2014 | 70 |
Al2O3 | DMAI | H2O | Silicon/glass | 100–300 °C | Patterned deposition | AS-s-ALD | 2014 | 70 |
AZO | DEZ/DMAI | H2O | Silicon/glass | 100–300 °C | Patterned deposition | AS-s-ALD | 2014 | 70 |
ZnO | DEZ | H2O | — | 200 °C | Patterned deposition | s-ALD | 2019 | 71 |
TiO2 | TTIP | N2/O2 plasma | Silicon/glass | 65 °C | Patterned deposition | PE-s-ALD | 2019 | 72 |
ZnO | DEZ | H2O | 3D printed substrates | — | Patterned deposition | s-ALD | 2020 | 73 |
TiO2 | — | — | 3D printed substrates | — | Patterned deposition | s-ALD | 2021 | 74 |
TiO2 | TTIP | H2O | — | — | Patterned deposition | s-ALD | 2021 | 75 |
ZnO | DEZ | H2O | — | — | Patterned deposition | s-ALD | 2021 | 75 |
TiO2 | TTIP | H2O | Silicon/aluminum/glass | 150 °C | Patterned deposition | s-ALD | 2021 | 76 |
ZrO2 | ZTB | H2O | Silicon/aluminum/glass | 150 °C | Patterned deposition | s-ALD | 2021 | 76 |
TiO2 | TTIP | H2O | Silicon | 120–260 °C | Patterned deposition | s-ALD | 2022 | 77 |
Pt | (MeCp)PtMe3 | O3 | Silicon | 200–250 °C | Patterned deposition | s-ALD | 2022 | 77 |
SiO2 | BDEAS | Ar/O2 | Silicon vs. ZnO/silicon | 100 °C | Patterned deposition | AS-s-ALD | 2023 | 78 |
Al2O3 | TMA | H2O | PET | 50 °C | Gas diffusion barrier | s-ALD | 2014 | 28 |
Al2O3 | TMA | Ar/O2 | Silicon/PET | 80 °C | Gas diffusion barrier | PE-s-ALD | 2016 | 79 |
Al2O3 | TMA | Ar/O2 | Silicon/glass | 75–150 °C | Gas diffusion barrier | PE-s-ALD | 2017 | 80 |
SnOx | TDMASn | O2/O3/H2O | Silicon/glass | 80–165 °C | Gas diffusion barrier | PE-s-ALD | 2018 | 81 |
ZnO | DEZ | H2O | Glass | 200 °C | Sensors | s-ALD | 2018 | 82 |
AZO | DEZ/TMA | H2O | Glass | 200 °C | Sensors | s-ALD | 2018 | 82 |
Al2O3 | TMA | H2O | Window glass | 50 °C | Wind shields | t-ALD | 2015 | 83 |
TiO2 | TDMAT | O3 | PDMS | 100 °C | Chemical stability | t-ALD | 2022 | 84 |
ZrO2 | TEMAZ | N2/O2 | Silicon/glass | 150–250 °C | MIMC | PE-s-ALD | 2017 | 85 |
AlxZn1−xO | DEZ/TMA | H2O | Glass | 200 °C | — | s-ALD | 2013 | 86 |
IZO | TMIn/DEZ | H2O | Glass | 200 °C | — | s-ALD | 2014 | 87 |
Ag | Ag(fod)(Pet3) | N2/H2 | Silicon | 100–120 °C | — | PE-s-ALD | 2015 | 88 |
Al2O3 | TMA | N2/O2 | Silicon | 20–100 °C | — | PE-s-ALD | 2016 | 89 |
ZrO2 | TEMAZ | N2/O2 | Silicon | 20–100 °C | — | PE-s-ALD | 2016 | 89 |
Al2O3 | TMA | H2O | Quantum dot films | 27 °C | — | t-ALD | 2016 | 90 |
Ag | (NHC)Ag(hmds) | Ar/H2 | — | 100 °C | — | PE-s-ALD | 2018 | 91 |
Al2O3 | Al(CH3)3 | Ar/O2 | Silicon | 80 °C | — | PE-s-ALD | 2019 | 92 |
ZnO | DEZ | H2O | Glass | 200 °C | — | s-ALD | 2021 | 93 |
Alucone | DMAI | EG | Silicon | 200 °C | — | MLD | 2022 | 94 |
Compared to other mixed metal oxides, ZnO-based oxides, especially amorphous semiconducting oxides such as IGZO, are the most widely studied for next-generation TFTs due to features including high mobility, excellent electric and chemical stability and the possibility for doping.45,100 The first study of ZnO-based TFTs by atmospheric-pressure s-ALD was authored by Levy et al.22,45 They deposited ZnO on top of the Al2O3 dielectric by a close-proximity s-ALD reactor. The ZnO-based TFTs thus prepared showed good performance with electron mobility approaching 20 cm2 V−1 s−1 and excellent stability. Later, the same group investigated the effect of cycle times on growth and transistor characteristics of ZnO deposited by atmospheric-pressure s-ALD. Once more, purge times are critical in optimizing the mobility of the TFT device. Electron mobility data as high as 22 cm2 V−1 s−1 have been realized for the ZnO-based TFTs grown at 200 °C with purge times as short as 25 ms without indication of a CVD component being present.46
In order to optimize and tailor the electronic properties of ZnO-based devices, doping is considered as an easy and efficient way achieved by atmospheric-pressure s-ALD.100 In s-ALD, doping can be easily realized by co-injecting the vaporized metal precursors into the deposition region. By adjusting the ratio of precursors, the properties of the resulted multicomponent oxides can be finely tuned. Commonly used dopant atoms for producing ZnO-based mixed oxide electronics are Al,86 In,87 N,95 and Mg.101 For example, Hoye et al.101 developed fluorene-free perovskite organometal halide light-emitting diodes (LEDs) by replacing the F8 electron injector with Mg-incorporated ZnO. The obtained LEDs had a higher luminance and lower turn-on voltages due to the reduced electron injection barrier of ZnO. By doping N in ZnO, Nelson et al.46 increased the sheet resistance of ALD-grown ZnO layers by more than an order of magnitude. To improve the mobility of TFTs, Illiberi et al.47 prepared indium zinc oxide (InZnO) using plasma-enhanced atmospheric-pressure s-ALD with trimethyl indium (TMIn), diethyl zinc (DEZ) and deionized water as precursors. The In/(In + Zn) ratio of the film was accurately tuned by varying their flows. The TFTs obtained at an In/Zn ratio of 2:1 showed a high mobility of over 30 cm2 V−1 s−1 and excellent stability.
The same authors also investigated the doping of both In and Ga into ZnO to prepare an amorphous oxide semiconductor (AOS). Amorphous IGZO is recognized as a promising material for the active channel in TFTs. The metal composition of IGZO was controlled by varying the flow of precursors. It was found that Ga-ions could hinder the formation of oxygen vacancies, suppressing the generation of free carriers and thus a decrease in field effect mobility with increased Ga-content was observed.43 Later, Katsouras et al.48 demonstrated the uniform deposition of IGZO on large substrates via the integration of an s-ALD-deposited Al2O3 buffer layer into the TFT stack. The final products showed low off-currents and field effect mobility of 9 cm2 V−1 s−1. More recently, Yoo et al.50 improved the performance of IGZO TFTs deposited on a polyimide substrate with an s-ALD-derived Al2O3 layer as the gate insulator. The field effect mobility of the IGZO TFT is as high as 52.5 cm2 V−1 s−1, while maintaining excellent bias reliability and mechanical bending stability.
Other mixed metal oxides have also been deposited with atmospheric-pressure s-ALD and explored as potential AOS materials for TFTs. For example, Mameli et al.51 reported the fabrication of p-type SnO-based TFTs with tin(II)-bis(tert-amyloxide), Sn(TAA)2, and H2O as the co-reactant by atmospheric-pressure s-ALD. Compared to conventional t-ALD, the deposition rates of SnO were up to 19.5 times higher when using atmospheric-pressure s-ALD. However, the linear mobility of the TFTs was only 0.4 cm2 V−1 s−1, which is lower than for the one deposited by t-ALD.102 Nguyen et al.49 demonstrated the deposition of SnO2 thin films by atmospheric-pressure s-ALD with tin(II) acetylacetonate (Sn(acac)2) and water as precursors. Due to the n-type nature of as-deposited SnO2, a high electron mobility of the films up to 11.2 cm2 V−1 s−1 was achieved.
To maximize their efficiency, solar cells are usually coated with an Al2O3 passivation layer with a proper thickness of typically ∼10 nm. Also, to realize mass production of solar cells for practical applications, high-throughput manufacture in a continuous process is a strict prerequisite.107 Here, the characteristics of low-cost, high-throughput and ease of scalability make atmospheric-pressure s-ALD an ideal candidate to fulfil these requirements in the PV industry.
Until recently, several thin-film materials have been tested and industrially employed for surface passivation of silicon solar cells such as silicon dioxide,108 silicon nitride109 and amorphous silicon.110 Compared to those materials, Al2O3 was demonstrated to be superior in increasing the efficiency of silicon solar cells drastically, as shown by the t-ALD work of Hoex and co-authors.111 This excellent surface passivation was attributed to the high negative fixed charge formed at the silicon/Al2O3 interface. Later, Poodt et al.54 demonstrated a high-quality and high-rate deposition of Al2O3 passivation films on silicon solar cells. Using atmospheric-pressure s-ALD they achieved extremely high growth rates up to 1.2 nm s−1 of the Al2O3 layers with excellent surface passivation. This concept has been commercialized by SoLayTec into a modular high-volume manufacturing tool, designed with 6 to 8 chambers yielding throughput numbers of more than 4000 wafers per h to meet industrial cost-efficiency requirement.54 Besides Al2O3 as a passivation cap layer, other functional materials have also been explored by atmospheric-pressure s-ALD to boost the efficiency of silicon solar cells. For example, Nguyen et al.68 studied the integration of Cu2O films as a hole-transporting layer in silicon heterojunction solar cells. The low-temperature deposited Cu2O films realized a power conversion efficiency of 13.7%, higher than other relevant studies. Here, the purity and stoichiometry of Cu2O is considered as key in maximizing the efficiency of solar cells since the presence of surface CuO was found to be detrimental.112
Beyond crystalline silicon, atmospheric-pressure s-ALD has also attracted the attention for the production of next-generation PV cells including CuInGaS (CIGS), organic and perovskite solar cells. The low production cost and high conversion efficiency (>21%) of CIGS solar cells make them gain increasing attention as the 2nd generation of PV. Typically, a buffer layer like CdS is used in CIGS solar cells to improve the overall efficiency. However, Cd is toxic and this drives researchers to explore other alternative materials. Zn(O,S), with a wider band gap than CdS, is considered an ideal replacing material. Interesting work on mixed oxysulfide (Zn(O,S)) functional layers with atmospheric-pressure s-ALD was published by Illiberi et al.57 They deposited Zn(O,S) buffer layers by exposing the substrate simultaneously to both H2O and H2S precursors, which were pre-mixed and co-injected in the same deposition zone. The effect of the S/(S + O) ratio on the optoelectronic and morphological properties of the Zn(O,S) layers was reported. A cell efficiency up to 15.9% was achieved at an optimum S/(S + O) ratio of about 0.4.59 This success prompted the researchers to transfer the Zn(O,S) deposition process to an industrial R2R s-ALD setup. An array of mini-modules with a surface area of 270 cm2 on a flexible substrate was demonstrated with a cell efficiency of 9.2%.65 The main advantage of organic solar cells lies in the flexibility of polymers, making them mass-manufacturable on various flexible substrate materials.113
Theirich et al.30 reported on the deposition of TiOx by plasma-enhanced atmospheric-pressure s-ALD at room temperature as the interlayer in inverted organic solar cells which performed similarly to those containing TiOx films prepared by conventional ALD or sol–gel processing.
Recently, research interest in solar cells has shifted towards perovskite-type cells due to their potential of reaching high energy conversion efficiency and low fabrication costs.64 Atmospheric-pressure s-ALD combined with R2R compatibility, would make up for a unique technology option.7 Najafi et al.64 employed a ZnO buffer layer to enhance the electron extraction in a perovskite solar cell structure. Improved efficiency and stability of the device were observed. Hoffmann et al.66 demonstrated ALD-grown SnOx as impermeable electron extraction layers for perovskite solar cells. The optical transmittance and electrical conductivity of the layer were similar to those reported for conventional ALD-grown layers.
Besides s-ALD, atmospheric t-ALD has also been demonstrated for several applications with planar substrates. One intriguing example is the deposition of Al2O3 films on the windshield of an automobile with a disk-shaped ALD delivery head in an open-air environment (Fig. 7).116 Another example is the coating of TiO2 films onto polydimethylsiloxane (PDMS) to enhance the organic solvent resistance of the materials.84
Fig. 7 Atmospheric t-ALD with a disk-shaped delivery head in an open-air environment. Reprinted with permission from Mousa et al.116 Copyright 2015, American Chemical Society. |
In s-ALD, the half-reaction zones are separated spatially, making the purging steps between the precursor dosages virtually obsolete.18 However, this cannot be readily achieved in t-ALD.
To increase the accumulated time-averaged deposition rates in t-ALD at atmospheric pressure, one trivial strategy is to drastically reduce the reactor volume, from liters (usual in t-ALD) to only milliliters in s-ALD, by narrowing the gap between the gas injection head to the substrate down to ∼100 to 200 μm. An additional measure to further prevent the mixing of precursors here is to increase the gas flow rate (for a minimized reactor volume). To this end, Jur and Parsons14 designed a unique ALD system in a flow tube geometry (with 60 cm length and 3.8 cm inner diameter) which offered the ability to adjust the process pressures independently and fixed at values between 2 and 760 Torr (Fig. 8a). To ensure sufficient exposure to the precursors during each self-limiting half-reaction under the high pressure and flow rate conditions, two separate inert gas streams were utilized. One stream pushes the precursors through a hold cell into the reactor at a fixed rate of 0.5 slm, while the other flows directly into the reactor to control the gas residence time. Based on simple gas kinetic models, a plot of gas residence time as a function of reactor pressure was obtained for two different values of gas flow rate (Fig. 8b). As expected, a transition from ALD (light shading) to CVD (dark area) region was observed. The analysis indicated that it is still possible to maintain good quality ALD regime at a pressure of 760 Torr by increasing the gas flow rate up to 5 slm. In addition, the authors illustrated experimentally the effect of the gas flow rate on GPC for the deposition of ZnO at 760 Torr (Fig. 8c). At atmospheric pressure and high gas flow (5 slm), the GPC of ZnO was the same as typical for the low-pressure ALD case. However, the GPC of Al2O3 was slightly larger than that at low pressure.
Fig. 8 (a) Schematic of a flow tube ALD reactor (60 cm length and 3.8 cm inner diameter) design which allows for the deposition at pressures varying from vacuum to atmospheric, (b) residence time vs. operating pressure of the flow tube, and (c) GPC of ZnO at 760 and 2 Torr, using 30 s purge times vs. purge gas flow rate. Reprinted with permission from Jur et al.14 Copyright 2011, American Chemical Society. |
To make fluidized-bed ALD more economically scalable, one can consider operation under atmospheric pressure for the coating of particles. This has received increased attention in recent years. Beetstra et al.,119 for the first time, tested atmospheric-pressure ALD of Al2O3 in a fluidized bed reactor to coat LiMn2O4 particles (200–500 nm) for battery applications, ranging from 5 to 28 cycles (Fig. 9a and b). The resulting coatings were characterized by transmission electron microscopy (TEM), energy dispersive X-ray (EDX) spectroscopy, scanning electron microscope (SEM) and X-ray diffraction (XRD). The results showed that the individual particles were coated homogeneously. Later on, Soria-Hoyo et al.122 demonstrated the potential of a scalable fluidized bed ALD reactor design for the production of a stable CO2 sorbent by coating CaO on a nano-silica powder matrix. The CO2 capture capacity of the coated materials was tested in a few cycles of thermogravimetric analysis (TGA). The results indicated that the synthesized materials were more stable than the limestone-derived CaO. In the same year, the group proposed a novel s-ALD reactor design consisting of a fluidized feeding vessel, a pneumatic transport line and a collection vessel, allowing the continuous production of nanoparticles at atmospheric pressure (Fig. 9c and d).121 More recently, the same group employed the fluidized bed ALD reactor to prepare photocatalytic core–shell samples with tunable activity via depositing an ultrathin layer of SiO2 on TiO2 nanoparticles.126 The deposition process was carried out at a temperature as low as 100 °C with silicon tetrachloride (SiCl4) as the precursor and H2O as the co-reactant. Surprisingly, a substantially lower chlorine impurity was observed in the deposited SiO2 layer which could hardly be achieved by low-pressure ALD.138,139 The photocatalytic property of the obtained TiO2/SiO2 nanostructures was proven by the degradation experiments with Rhodamine B (RhB) solution. The results suggested that the highest photocatalytic activity of the particles was achieved at a SiO2 layer thickness of 0.7 nm. Conversely, the performance of the photocatalyst was strongly suppressed when the SiO2 layer was thicker than 1.4 nm.
Fig. 9 Atmospheric-pressure ALD on high-porosity particles. (a) fluidized bed ALD reactor to particle coating, (b) TEM image of a particle obtained by fluidized bed ALD, (c) schematic of the s-ALD reactor consisting of a fluidized feeding vessel, a pneumatic transport line made of three segments: preheating (i), precursor reaction zone (ii), co-reactant reaction zone (iii), and a collection vessel, (d) TEM image of Pt/TiO2 samples obtained by s-ALD. Reprinted with permission from Beetstra et al.119 and Van Ommen et al.121 |
Another important application of fluidized-bed ALD is in the pharmaceutical domain. The ability to obtain pharmaceutical particles with tailor-made size, shape and surface properties has significant implications for drug delivery and therapeutic applications. Zhang et al.128,129 demonstrated the successful, complete and conformal layering of Al2O3 films on drug particles in a fluidized ALD reactor at near-atmospheric pressure. With a few ALD cycles, the properties of drug particles such as their dissolution, dispersibility and heat transfer can be improved and this way the release and utilization of ALD-modified drug particles can be further optimized. Also, La Zara et al.130 compared the effect of different coatings, including ALD-grown Al2O3, TiO2, SiO2, and MLD-grown PET and titanicone, on the wettability of drug particles. The ceramic ALD films were most effective in improving the hydrophilicity of the drugs while PET films, made by molecular layer deposition (MLD) – the organic counterpart of ALD, were effective in delivering hydrophobic powders.
Overall, potential applications of nanoparticles developed by fluidized-bed atmospheric-pressure ALD in various areas are listed in literature (Table 3). Developing fluidized bed reactors for ALD at an industrial scale is expected to be viable and in addition, to be much more convenient under atmospheric pressure.137 However, one can also expect that high-humidity air flows entering the reactor, may lead to unwanted side reactions. This is especially important when the second precursor being used is water.
Materials | Precursor | Co-reactant | Substrate | Deposition temperature | Applications | ALD type | Year | Ref. |
---|---|---|---|---|---|---|---|---|
Cp = cyclopentadienyl; Me = methyl; thd = 2,2,6,6-tetramethyl-3,5-heptanedionato; PET = poly(ethylene terephthalate); TC = terephthaloyl chloride; MLD = molecular layer deposition; EG = ethylene glycol; hfac = hexafluoroacetyl-acetonate; GC = gas chromatography; RT = room temperature; — = not mentioned.a See also Fig. 9 for illustrations. | ||||||||
Al2O3 | TMA | H2O | Particles | 160 °C | Li-ion batteries | t-ALD | 2009 | 119 |
Pt | MeCpPtMe3 | O3 | Particles | 250 °C | Catalysis | t-ALD | 2013 | 120 |
Pt | MeCpPtMe3 | O2 | Particles | 100/250 °C | Catalysis | s-ALD | 2015 | 121 |
CaO | Ca(thd)2 | O3 | Particles | 250 °C | CO2 capture | t-ALD | 2015 | 122 |
Al2O3 | TMA | H2O | Particles | 27 ± 3 °C | — | t-ALD | 2015 | 123 |
Pt | MeCpPtMe3 | Air | Graphene | 100 °C | Catalysis | t-ALD | 2017 | 124 |
Cu2O | Cu(I)(hfac) | H2O | Particles | 250 °C | Photocatalysis | t-ALD | 2021 | 125 |
SiO2 | SiCl4 | H2O | Particles | 100 °C | Photocatalysis | t-ALD | 2020 | 126 |
PET | TC | EG | Particles | 150 °C | Photoactivity | MLD | 2020 | 127 |
Al2O3 | TMA | H2O | Particles | 100 °C | Drug delivery | t-ALD | 2017 | 128 |
Al2O3 | TMA | O3 | Particles | 30 °C | Drug delivery | t-ALD | 2019 | 129 |
Al2O3 | TMA | O3 | Particles | 40 °C | Drug delivery | t-ALD | 2021 | 130 |
TiO2 | TiCl4 | H2O | Particles | 40 °C | Drug delivery | t-ALD | 2021 | 130 |
SiO2 | SiCl4 | H2O | Particles | 40 °C | Drug delivery | t-ALD | 2021 | 130 |
PET | TC | EG | Particles | 150 °C | Drug delivery | MLD | 2021 | 130 |
Titanicone | TiCl4 | EG | Particles | 120 °C | Drug delivery | MLD | 2021 | 130 |
Al2O3 | TMA | H2O | Particles | 180–300 °C | — | t-ALD | 2021 | 131 |
Al2O3 | TMA | H2O | Capillary column | 300 °C | GC | t-ALD | 2022 | 16 |
TiO2 | TiCl4 | H2O | Membrane | 180 °C | Water treatment | t-ALD | 2017 | 132 |
ZnO | DEZ | H2O | Membrane | RT | Separation | s-ALD | 2022 | 133 |
Al2O3 | TMA | H2O | Cotton fabric | 100 °C | — | t-ALD | 2011 | 14 |
A few commercial companies working on the coating of nanoparticles with atmospheric-pressure ALD are worthwhile mentioning. One start-up company, Delft IMP, is dedicated to commercializing its ALD and MLD technologies for depositing ultrathin layers on powder surfaces, particularly for energy transition applications like batteries, catalysts, fuel cells and electrolysers.140
On a parallel track, Forge Nano has developed and commercialized a continuous vibrating bed ALD reactor named ‘CIRCE’.141 This reactor is designed for s-ALD mode mass production at atmospheric pressure with a high production capacity up to 4000 kg h−1 and >99% product yield. The reactor can be used at temperatures ranging from 50 to 200 °C, making it suitable for various kinds of particles and coating materials.
Fig. 10 (a) Schematic overview of flow-through atmospheric t-ALD for the deposition of Al2O3 on the capillary column, (b) measured Al2O3 thickness grown on silicon in two different chambers after different numbers of ALD cycles, and TEM images of the respective film thickness at the entrance (c) and end (d) of the capillary column after 100 ALD cycles. From Patel et al.16 Copyright 2022, American Chemical Society. |
In this regard, researchers have studied the potential of using both atmospheric-pressure t-ALD and s-ALD for membrane fabrication and modification. For example, Shang et al.132 prepared tight ceramic NF membranes by a flow-type atmospheric-pressure t-ALD reactor (Fig. 11a). Two commercial ceramic NF tubes were vertically placed in an up-flow reactor and a silicon wafer was fixed as a reference sample next to the membrane to monitor the thickness of the coated layer. The molecular weight cut-off (MWCO) of the membranes was reduced to a range of 260 to 380 Da from an initial value of 450 Da after one to three cycles of TiO2 coating from TiCl4 and water vapor. However, a high water permeability (11–16 L m−2 h−1 bar−1) of these modified ceramic membranes was maintained, which is notably higher than commercial polymeric membranes and sol–gel-made ceramic NF membranes with a similar MWCO (∼300 Da). The growth rate of the layer was found to be much smaller than the one deposited at the planar silicon surface, which could be ascribed to the steric hindrance of the TiCl4 molecules into the pores of NF membranes. In another study, Toldra-Reig et al.133 explored the deposition of thin ZnO films on tubular ceramic membranes by designing and fabricating a customized 3D-printed s-ALD manifold (Fig. 11c). To ensure a homogeneous deposition on the membrane surface, the geometry of the gas manifold was optimized by CFD simulation prior to design. The deposition of the ZnO layer with such a gas manifold was validated on both a tubular Cu foil and a porous Al2O3 tubular membrane. The results indicated that s-ALD is a promising route for high-rate deposition of high-quality conformal thin films on complex substrates. However, due to a major CVD contribution, the GPC of the ZnO layer was measured to be 4 Å per cycle, which is much higher than that of the conventional ALD. In addition, the membrane properties such as pore size and water permeance were not yet investigated in this study. Furthermore, the manifold design used only allows for the deposition of ALD layers on the outer surface of the membrane, making it hard to be compatible with commercial multichannel ceramic membranes.
Fig. 11 Atmospheric-pressure ALD for membrane modification. (a) Schematic overview of a t-ALD setup, (b) MWCO of membranes before and after ALD modification; (c) photograph of an atmospheric s-ALD setup, and (d) configuration of its injection head for the growth of ZnO on the outer surface of a ceramic Al2O3 tubular membrane, and cross-section micrograph of the grown ZnO film. From Shang et al.132 and Toldra-Reig et al.133 (Copyright 2022, American Chemical Society). |
(1) |
The mean free path λ of molecules is mainly affected by three key factors: temperature T (K), molecule size d (m) and pressure p (Pa). To describe their relationships, the following equation is given:
(2) |
Given the above theoretical equations, two flow regimes can be separated based on the mean free path, the pore diameter of the substrate and the pressure of the system, as shown in Fig. 12. In the viscous flow regime (Kn ≪ 1), the mean free path of the molecules is much smaller than the pore diameter of the substrates. In this case, inter-particle interactions dominate the transport process. On the contrary, in the molecular flow regime (Kn ≫ 1) the mean free path of the molecules is much larger than the pore diameter of the substrates, leading to particle–surface interactions as the main transport phenomenon. Therefore, in very low pressure condition (pump-type reactor), molecular flow can be easily achieved even in macroscopic structures. Thus, in a conventional temporal ALD reactor, molecular flow can often be obtained on porous substrates with macropores. Whereas, at near-atmospheric pressures, the molecular flow will only be realized in nanopore structures.152
Fig. 12 Mean free path (left y-axis) as a function of pressure, calculated according to eqn (2), for molecules with average diameters of 5, 7, and 9 Å, respectively, at a temperature of 100 °C. The working pressure regimes of the pump-type, flow-type, and atmospheric pressure (AP-type) ALD reactors are indicated in the figure. The right y-axis of the graphs shows the characteristic feature size (dp). Comparing dp with the mean free path, λ, allows determination of the corresponding flow regime for a given pressure: molecular flow regime (λ ≫ dp) and viscous flow regime (λ ≪ dp). From Cremers et al.152 |
(3) |
The molecular diffusion coefficient (DM) is only pressure dependent, thus irrelevant to the pore size of the substrate. In other words, the diffusion coefficient is increased with decreasing pressure, and vice versa. On the contrary, the Knudsen diffusion coefficient (DKn) is dependent on the pore size of the substrate and independent of the overall pressure. With these three parameters (the molecular, Knudsen, and effective diffusion coefficients), one can plot these for a precursor either as a function of pore size at atmospheric pressure or as a function of reactor pressure for a certain pore size (Fig. 13).
Fig. 13 Diffusion coefficients of TMA as a function of (a) pore size at a fixed pressure of 105 Pa, and (b) reactor pressure for a fixed pore size of 1 μm. From Poodt et al.153 |
If we take TMA as an example, it can be seen that Knudsen diffusion still dominates when the pore size of the substrate is smaller than 0.5 μm at atmospheric pressure (Fig. 13a). For a 1 μm diameter pore, Knudsen diffusion prevails at a reactor pressure of up to 104 Pa (Fig. 13b).
Next, the saturation dose of a precursor required to completely cover the walls of a pore can be estimated by including the pressure-dependent diffusion coefficient (Deff) in the model of Gordon et al.154 Exposure of a substrate to a certain gas dose is determined by the product of its partial pressure and the exposure time. Therefore, for a given pore structure with known pore size and pore length, the saturation dose and saturation time can be mathematically calculated for different pressures. In their study Poodt et al.153 found that, for a 1 μm diameter and 50 μm deep circular pore, the saturation time could be 10 times less at atmospheric pressure as compared to a low-pressure condition (133 Pa), although the saturation dose could be 2 times higher. In atmospheric-pressure ALD, a much higher precursor partial pressure is allowed, and thus shorter saturation times can be achieved than for low-pressure ALD. To further demonstrate the feasibility of atmospheric-pressure ALD for conformal coating on substrates with macropores, Poodt et al.153 coated a silicon wafer substrate with 17 μm deep pores of 1 μm diameter created by a Bosch-type Deep Reactive Ion Etching (DRIE) process. To make sure that a near-to-complete step coverage was achieved, a long precursor exposure time (∼250 ms) per cycle was used (cf. 10 ms for planar substrates). As shown in Fig. 14, for such a high aspect ratio structure, conformal coating (100% step coverage) was successfully realized with s-ALD at atmospheric pressure despite that molecular diffusion dominates in this pore dimension.
Fig. 14 Cross-sectional SEM images of 1 μm diameter and 17 μm deep pores array in silicon, conformally coated by atmospheric ALD of Al2O3. (a) Global structure, (b) pore opening and (c) pore bottom. From Poodt et al.153 |
The conformal coating of thin films on high aspect ratio substrates at atmospheric pressure was also confirmed by Roozeboom et al.155 In their study, arrays of trenches with an aspect ratio as high as 138:1 were used for the deposition of an Al2O3 layer from TMA and H2O. In such a high aspect ratio structure with 65 nm trench openings and 9 μm trench depth, the conformal coating was realized at 1 atm. and 200 °C in a rotatory s-ALD reactor with a cycle time of 13.5 ms (Fig. 15).
Fig. 15 Cross-sectional SEM images of an Al2O3 layer deposited at 1 atm. and 200 °C in 138:1 aspect ratio trenches during 600 cycles in a rotary s-ALD reactor. (Trenched wafers kindly provided by Fraunhofer CNT/Namlab, Dresden). From Roozeboom et al.155 |
Overall, for small pore diameters, Knudsen diffusion dominates the transport of molecules, even for atmospheric-pressure ALD. As a result, the saturation dose is the same for both low- and high reactor pressure. Whereas, in terms of large pore diameters, higher saturation doses are required for high-pressure reactors than for low-pressure reactors. Benefiting from the high precursor partial pressure, the saturation time of the precursor is even shorter for atmospheric ALD than for low-pressure ALD.
George and co-workers were one of the first to develop an ALD reactor system which allows for in situ monitoring of pore size variation of a tubular Al2O3 membrane with the number of ALD cycles.156,157 The initial pore size of the membrane was 50 Å and the pore diameter reduction was monitored using in situ N2 and Ar permeation measurements. By assuming Knudsen diffusion and using an aperture pore model, the pore size of the membrane can then be estimated by permeation results. The authors investigated the Al2O3 membrane coating with ALD Al2O3, SiO2, and TiO2, and found the pore diameter reduction rates to vary among these materials. This could be partially explained by the different deposition temperatures and thus the different hydroxyl surface group concentrations present on the material surface. In addition, the final pore diameters may reach a minimum value which is defined by the molecular size of the reactant or the molecular size of the gases used for permeation measurements. These results demonstrated the potential of ALD in tailoring nanopores of membranes for specific applications.
With in situ gas permeation measurements, however, only the information on pore size variations can be obtained. To gain more information (e.g., porosity and pore size distribution) about the penetration of ALD coatings into substrates with mesopores and/or nanopores, Dendooven et al.158–162 developed several approaches by implementing in situ characterization into an ALD reactor. As shown in Fig. 16, in situ X-ray fluorescence (XRF) was employed to monitor the Ti uptake during the deposition of TiO2 in mesoporous films with an initial average pore size of 4 nm as well as on a planar SiO2 surface.161,162 The Ti XRF intensity from the mesoporous substrate increased much faster than the one deposited on a planar SiO2 substrate in the first few cycles, suggesting the penetration and deposition of an ALD layer inside the mesopores. With the increase of ALD cycles, the intensity increase of the Ti-signal from the mesoporous film slowed down due to the narrowing down of pore width as well as the decrease of accessible interior surface area. After a certain number of cycles, the slope of the Ti-intensity curve became constant, indicating that the deposition continued only on top of the outer surface as the pores were completely filled with TiO2. Also, the ALD reactor could be integrated with other in situ characterization methods such as ellipsometric porosimetry (EP)160 and grazing incidence small-angle X-ray scattering (GISAXS).158 This way, EP could provide information on the porosity and pore size distribution during the ALD growth on mesoporous or nanoporous features, and with GISAXS one could monitor the evolution in density and internal surface area as growth progresses. Especially with the combination of such advanced in situ characterization techniques, better insights on the pore-filling mechanism can be obtained.158,159
Fig. 16 Normalized Ti XRF intensity as a function of the number of TiO2 ALD cycles on a planar SiO2/Si substrate and on a mesoporous substrate with an initial average pore size of 4 nm. The cartoons display the gradual pore filling until completion followed by surface growth only. From Dendooven et al.161 |
Currently, in situ characterization techniques of ALD layers grown on porous substrates are typically available in low-pressure ALD reactors only. However, some techniques can be expected to be more easily integrated into atmospheric-pressure ALD reactors. For example, the in situ N2 and Ar permeation measurements are easier to be achieved since no vacuum system is required.
Fig. 17 (a) Schematic top view and (b) computational flow dynamics simulation of the gas injectors in the Encapsulix parallel precursor wave (PPW) system. (c) Iso-contour lines for precursor pulsed wave fronts after propagation of the precursor pulses in the reaction space.163 |
Most of the reactor design and process aspects described above can be traced back, amongst others, to the early and fundamental work published by Giling,164 who investigated gas flow patterns in several horizontal reactor designs by interference holography. In general, the flow patterns and their stability while propagating from the entrance to the outlet of a reactor are mainly impacted by three factors: (1) the occurrence of turbulence due to (too) high gas flow rates, (2) the occurrence of thermal convection as a result of temperature gradients along the reactor height axis which can disturb laminar flow regime, and (3) any reactor entrance and outlet effects causing undeveloped flow and temperature profiles. For example, Giling reported that the thermal entrance length should often be several times longer than the flow entrance length. These thermal entrance effects should be taken into account in developing new reactor designs, in terms of optimized inlet length, adding a preheating zone and optimizing the free height of a reactor. In occasional cases, carrier gases with a high thermal capacitance, like H2 and He are easier in establishing stable laminar flow compared to N2 and Ar.164 However, they are less cost-effective.
Each application requires a specific reactor design optimized for its intended purpose. For example, large-area/foil substrates (e.g., solar cells and displays), require a R2R design, while single-wafer ALD is suitable for rigid wafers. Powder coating necessitates a fluidized-bed design, whereas flow-through or shower head designs are preferable for other applications. The design of each concept is tailored to meet the specific demands of the electronics industry and the unique characteristics of different substrates, such as their porosity.
In addition, considerations on flow dynamics at high vs. low operation pressure and challenges and opportunities associated with the reactor design are included, as well as some recent highlights in patterned deposition and Molecular Layer Deposition.
Footnote |
† Present address: Department of Chemical Engineering, Delft University of Technology, 2629 HZ Delft, The Netherlands. E-mail: m.chen-1@tudelft.nl |