Antonella Rozaria Nefeli
Pontillo
a,
Spyridon
Koutsoukos
b,
Tom
Welton
b and
Anastasia
Detsi
*a
aLaboratory of Organic Chemistry, Department of Chemical Sciences, School of Chemical Engineering, National Technical University of Athens, Zografou, Greece. E-mail: adetsi@chemeng.ntua.gr
bDepartment of Chemistry, Molecular Sciences Research Hub, Imperial College London, White City Campus, London W12 0BZ, UK
First published on 10th May 2021
In the present work, the plasticising effect of the natural deep eutectic solvents (NaDESs) choline chloride/lactic acid and betaine/lactic acid in the formation of chitosan-stabilised films is investigated. The films were prepared by the casting technique, dissolving chitosan in 1% w/v solution of choline chloride and lactic acid or betaine and lactic acid in water, either as a pre-formed NaDES or as separately added components (physical mixture), without the addition of acetic acid. The physicochemical and mechanical properties of the formed films were studied. High concentration of the NADES (83%) increases the weight and thickness of the films. The reference chitosan films containing acetic acid or lactic acid are inelastic and very resistant to burst. On the other hand, the addition of betaine increases significantly the elongation capacity of the film prior to burst. The water vapour permeability of the films prepared from the NaDES solutions presents a 4.5 and a 2.6-fold increase, respectively, in comparison with acetic acid containing films. The materials prepared using the NaDESs have distinct differences to those prepared using the physical mixture of the NADESs’ components, as shown from the thermal and FT-IR spectroscopic analyses data. Finally, SEM imaging revealed differences among the surfaces of the films.
The gelation of NaDESs has only recently been reported and proposed for a variety of different applications. Xia et al.10 investigated choline chloride-xylitol NaDES, employing xanthan gum as the gelation agent. The ability of the NaDES to dissolve bioactive compounds like quercetin, renders the so-called eutectogels as a promising alternative for oral and transdermal drug delivery. Marullo et al.11 prepared choline chloride–phenylacetic acid eutectogels using different amino acids as gelators. The study revealed that the prepared formulations could be used as sorbents for the removal of dyes from wastewater with high removal efficiency and recyclability.
Chitosan exhibits strong antimicrobial and antifungal activity.12,13 Due to their inherent non-toxic and biodegradable nature, chitosan films are considered as versatile alternatives to conventional plastic polymer films, which could find use in numerous applications. In the food industry, chitosan films have been investigated as packaging material to prolong the shelf-life of products.14 In the pharmaceutical industry, their use as wound dressings is being investigated, as they could incorporate a therapeutic agent offering a controlled release and enhancing its properties.15,16
The mechanical properties such as the elasticity and tear resistance of different films can be varied significantly, depending on the requirements of each application. Flexibility and pliability are essential properties for wound dressings in order to cover the wound and prevent infection.17,18 On the other hand, a packaging material may be flexible or inelastic to maintain its integrity throughout the transportation and storage of the products.19,20
Water vapour permeability (WVP) is a significant property of films. Water vapours transfer through a film by absorption, diffusion through the film due to interaction with the polymer and desorption.21 All films are permeable, but depending on their structure, some may create a stronger barrier. The requirements of the application define the selection of polymers and additives. For instance, in food packaging, research is oriented towards decreasing the permeability of water through the film, thus protecting the shelf life of packaged products, as water causes bacterial development and, consequently, spoilage of the aliments.22–24 On the other hand, the permeability of water through wound dressings should not be too low as the healing time and the risk of bacterial infection increases,25,26 nor too high as it may cause dehydration of the area and subsequently, a scar.27,28
In spite of its remarkable bioactivity and extent of potential applications, chitosan presents an inherent difficulty to dissolve in any solvent apart from acidic aqueous solutions (most commonly 1% acetic acid). In an effort to explore additional options regarding chitosan's solubility and film-making ability, in the present work, we investigated the solubility of chitosan in aqueous solution of two selected NaDESs namely choline chloride:lactic acid (ChCl:LA 1:1.5) and betaine:lactic acid (bet:LA 1:2) and demonstrated that chitosan can be dissolved in solutions of 1% w/v NaDESs in water and, thus, elastic films were prepared via the casting technique.
According to the experimental and computational work of Gutiérrez et al.,29 large dilutions of a NaDES disrupt the intermolecular interactions between the components. Therefore, it is theoretically expected that a 1% aqueous solution of a NaDES is equivalent to an aqueous mixture of its components.
In order to comprehend whether the pre-formation of the NaDES has an impact on properties of the films, two different films were prepared for each NaDES. For the first film, the NaDES was synthesised and dissolved in water, while for the second film, the appropriate amounts of the two components were directly dissolved in water, prior to chitosan addition. Subsequently, the water was evaporated, forming the following films: F/ChCl:LA NADES and F/ChCl:LA mix. and F/bet:LA NaDES and F/bet:LA mix., respectively. The addition of acetic acid was not required in any of the films, as the formed aqueous solution was already acidic.
Moreover, the effect of lactic acid (LA) was also monitored in two different concentrations, first 0.4% (F/0.4LA), equivalent to the concentration of LA in 1% ChCl:LA NaDES, and 0.5% (F/0.5LA) equivalent to the LA in 1% of the bet:LA NaDES. Finally, the results were compared with films produced with the addition of the well-known plasticiser Tween 80 (F/Tween).
Film | Weight (mg) | Thickness (mm) |
---|---|---|
F/AA | 113.76 ± 4.3 | 0.037 ± 0.005 |
F/Tween | 183.04 ± 6.8 | 0.081 ± 0.020 |
F/bet:LA NaDES | 495.40 ± 15.0 | 0.152 ± 0.070 |
F/bet:LA mix. | 465.63 ± 9.7 | 0.110 ± 0.010 |
F/0.5LA | 217.70 ± 16.8 | 0.057 ± 0.020 |
F/ChCl:LA NaDES | 518.76 ± 9.4 | 0.126 ± 0.019 |
F/ChCl:LA mix. | 487.33 ± 15.5 | 0.105 ± 0.003 |
F/0.4LA | 209.45 ± 11.2 | 0.052 ± 0.020 |
The films prepared from the NaDES solutions (F/bet:LA NaDES and F/ChCl:LA NaDES) are significantly thicker than the corresponding films prepared from the LA solution (F/0.5LA and F/0.4LA). A plausible explanation is that the presence of the betaine or the choline chloride moiety provides an additional spacing between the chitosan chains as these molecules can form additional hydrogen bonds and electrostatic interactions with the polymer functional groups which results in the swelling of the film.
On the other hand, the NaDES-containing films appear to be only slightly thicker than the films containing the components of the NaDES when they are added as a mixture.
The impact of the acid on the films’ mechanical properties was again confirmed: the presence of lactic acid instead of acetic acid increases both the BS and the DB of the films. Moreover, a higher concentration of lactic acid has a strong effect on the BS of the films, while the DB remains practically the same. Therefore, the lactic acid containing films (F/0.5LA and F/0.4LA) are more elastic, yet more difficult to break than the acetic acid film (F/AA). This observation is in accordance to the work of Caner et al.21 On the other hand, the films prepared from the NaDES solutions (F/bet:LA NaDES and F/ChCl:LA NaDES) presented significantly lower resistance to rupture, but were more elastic compared to the reference films. The films formed from the NaDES solution or from the solution containing the mixture of the two components of the NaDES, required 86–95% less burst strength to be ruptured while their ability to elongate was 13–78% higher than the corresponding films formed from the solutions of the acids.
The plasticising effect achieved in the films F/bet:LA NaDES, F/bet:LA mix., F/ChCl:LA NaDES and F/ChCl:LA mix. is clearly observed in Fig. 2. Higher elasticity is expected with the addition of NaDESs, as the free space between the polymeric chains is increased.37 Hence, the DB of F/bet:LA NaDES and F/ChCl:LA NaDES is increased to 20.1 mm and 11.0 mm respectively while for F/AA is 4.8 mm.
Moreover, the F/bet:LA mix. and F/ChCl:LA mix. presented similar elongation ability prior to burst as the F/bet:LA NaDES and F/ChCl:LA NaDES respectively, suggesting that the addition of the two components separately or as a pre-formed NaDES does not affect the mechanical properties of the films.
Another interesting observation is that both betaine containing films were noticeably more elastic than F/ChCl:LA NaDES and F/ChCl:LA mix.
The highly hydrophilic character of choline chloride promotes the water vapour diffusion. Therefore, the choline chloride containing films exhibit the highest WVP.37
As can be observed from Fig. 3, when the two components of the NaDES are added separately in the film forming solution, the WVP is lower compared to the films where the NaDES was synthesised prior to the chitosan dissolution. A plausible explanation could be that when the components of the NaDES are separately added, they are more uniformly incorporated between the chitosan chains. This could be attributed to the hydrogen bonds of the NaDES, resulting in higher swelling of the polymer, enlarging the spacing formed between the polymer chains and permitting the permeant water vapour to pass through more easily. If the existence of NaDES causes the formation of hydrogen-bonded, water-friendly, clusters between the chitosan chains, then these clusters could easily act as passages for water to enter the film WVP of aluminum foil, a strong barrier of water, was measured as reference.
The spectrum of F/Tween (Fig. 4) reveals that Tween 80 does not chemically interact with chitosan, as there are only minor peak shifts compared to the neat Tween 80 spectrum.40
From the spectra of F/0.4LA and F/0.5LA (Fig. 5) it can be observed that the peaks in the range 3600 to 3000 cm−1, as well as the peaks from the CO stretching vibration of the COOH group (present at 1721 cm−1 in the spectrum of F/0.4LA and at 1722 cm−1 in the spectrum of F/0.5LA) are significantly more intense than in the spectrum of F/AA. This indicates that the excess of lactic acid remains in the system in its neutral form, as it is less volatile than the acetic acid. The two bands at 2982 cm−1 (CH2 vibrations) and 2521 cm−1 (–OH stretching) correspond to the lactic acid. Moreover, the band at 1566 cm−1 or 1570 cm−1, respectively, is attributed to the antisymmetric –COO− stretching vibration of the lactate ion, which has been shifted due to the presence of the electron-withdrawing –OH group in the 2-position. Furthermore, a new small shoulder appears at 1521 cm−1, corresponding to the ammonium cation, verifying the formation of chitosan lactate.41–43
In the spectrum of F/bet:LA NaDES (Fig. 6) the bands at 2923 and 2854 cm−1 are very strong, while the 3412 cm−1 peak is significantly weaker and the –OH peak is negligible, indicative of a smaller amount of the acid in its neutral form. Moreover, the –COOH and the –COO− peaks are now reversely intense, as the carboxyl groups are consumed, indicating the formation of lactate ion.
For the F/bet:LA mix. (Fig. 6) the peak at 1727cm−1 is of significantly lower intensity than the 1619 cm−1 peak, indicative of a greater amount of lactic acid in its neutral form compared to the F/bet:LA.44,45
The FT-IR spectra of F/ChCl:LA NaDES and F/ChCl:LA mix. (Fig. 7) present broad strong peak at around 3323 cm−1 and 3323 cm−1 respectively attributed to the O–H and N–H stretching vibrations. The absorbance from the carboxyl group of LA is observed at 1731 cm−1 in the F/ChCl:LA NaDES spectrum and is shifted by 2 cm−1 in the F/ChCl:LA mix. spectrum. The absorbances at 1479 and 1480 cm−1, respectively, are attributed to –CH2 scissoring, and the peaks at 1127 and 1128 cm−1 are attributed to the C–C stretching vibration.43,46
The FT-IR spectra of the NaDESs bet:LA and ChCl:LA are presented in Fig. S2 (ESI†).
All samples present a wide set of peaks in the range 1200–1000 cm−1, with different behaviour for each sample. These peaks have been deconvoluted, by fitting Gaussian functions, in order to reveal overlapping peaks (Fig. S3–S9, ESI†) while the Gauss Curve equation parameters are explained in Fig. S10 (ESI†). The accuracy of the Gaussian fitting can be seen at Tables S1–S7 in the ESI.†Table 2 summarises the revealed peaks of all samples in the studied range.
Sample | Peak 1 (cm−1) | Peak 2 (cm−1) | Peak 3 (cm−1) | Peak 4 (cm−1) | Peak 5 (cm−1) |
---|---|---|---|---|---|
F/AA | 1150 | — | 1076 | — | — |
F/Tween | 1149 | 1127 | 1078 | 1024 | — |
F/0.5LA | — | 1124 | 1079 | 1030 | 1001 |
F/bet:LA NaDES | — | 1126 | 1082 | 1035 | 1015 |
F/bet:LA mix. | — | 1127 | 1079 | 1030 | 1001 |
F/ChCl:LA NaDES | — | 1126 | 1082 | 1043 | 1004 |
F/ChCl:LA mix. | — | 1126 | 1082 | 1040 | 998 |
From Table 2, it can be seen that in both samples containing acetic acid, a peak at 1150/1149 cm−1 appears, corresponding to the C–C stretching vibration of the acid (Peak 1). However, when lactic acid is present in a film, the band is shifted towards lower wavenumbers. For the F/Tween, both bands appear, Peak 1 corresponding to the acid and Peak 2 corresponding to the plasticiser. Peak 3 (C–O) appears in all samples as well as in the raw chitosan spectrum. Peak 4, is characteristic of the lactic acid, although slightly shifted from that reported in literature (1043 cm−1). Peak 5 differs among the studied samples, probably because it is due to different interactions. For F/bet:LA NaDES and F/bet:LA mix. Peak 5 corresponds to the R-N(CH3)3+ skeletal vibrations, while for F/0.5LA it corresponds to C–H or C–O vibrations (rocking, deformation, stretching).
The interesting observation in this range, is that the relative intensities of the peaks differ between samples. For F/bet:LA NaDES Peak 2 is the strongest, while in F/bet:LA mix. and F/0.4LA the Peaks 3 and 4 are stronger than Peak 2. This could be explained with a higher amount of lactic acid existing in its neutral form, thus, it could be supposed that the salt formation is hindered in the case of F/bet:LA NaDES. This could also be verified by the relative intensities of the 1730 and 1622 cm−1 peaks (1727 and 1619 cm−1, respectively, in the mixture): in F/bet:LA NaDES the difference in intensity is much smaller than in F/bet:LA mix., although the amounts of each component are the same.
Similarly, the comparison of the relative intensity of Peaks 2, 3 and 4 between the F/ChCl:LA NaDES and F/ChCl:LA mix. spectra indicates the lower amount of free lactic acid in the former sample.
Having established that the interaction between chitosan and each acid occurs towards the formation of the corresponding salt, it has been confirmed that the excess of acetic acid evaporates during the film formation while lactic acid remains in the system. Furthermore, the addition of lactic acid as a component of a preformed NaDES into the system ‘protects’ the lactic acid in its neutral form. This results in the reaction with fewer amino groups of chitosan in contrast to the mixture of the components, in which the expected chemical equilibrium is maintained. Therefore, there is an indication of different chemical environments existing in the samples, which could be responsible for the differences observed in the thermal and mechanical properties of the films.
Sample | TGA moisture content (% weight) | T onset (°C) | T max.rate (°C) | T 1/2 (°C) | Residue (% weight) |
---|---|---|---|---|---|
bet:LA NaDES | 4.4 | 192 | 249 | 243 | 3.4 |
ChCl:LA NaDES | 5.5 | 194 | 262 | 253 | 1.2 |
F/AA | 9.1 | 200 | 278 | 280 | 25.2 |
F/Tween | 5.0 | 247 | 429 | 380 | 11.4 |
F/bet:LA NaDES | 6.3 | 201 | 250 | 249 | 6.5 |
F/bet:LA mix. | 6.4 | 211 | 255 | 252 | 1.0 |
F/0.5LA | 4.8 | 163 | 178, 283 | 261 | 12.0 |
F/ChCl:LA NaDES | 8.2 | 225 | 268 | 262 | 5.1 |
F/ChCl:LA mix. | 8.3 | 209 | 273 | 258 | 3.6 |
Chitosan | 3.0 | 272 | 294 | 299 | 36 |
Acetic acid | — | — | — | — | — |
Lactic acid | 12.9 | 145 | 179 | 188 | 0.3 |
Betaine | 0.9 | 295 | 302 | 302 | 1.8 |
Choline chloride | 1.8 | 303 | 307 | 307 | 1.0 |
F/AA shows decomposition throughout the heating range (Tonset = 200 °C), which results in 25 wt% carbon residue (Fig. S12, ESI†). As expected, chitosan decomposes mainly to H2O (m/z = 18) and CO2 (m/z = 44). This can be confirmed from the MS spectra of the neat polymer (Fig. S19, ESI†). Spectra with m/z = 16 and 32, which correspond to atomic and molecular oxygen, show a continuous reduction in intensity, as the MS column is flushed with N2 through the measurement, removing the trapped oxygen. No oxygen seems to be produced during the decomposition of chitosan. The graph for m/z = 29 is interesting, as it shows an initial reduction, followed by a constant production in the range 300–500 °C, which indicates that although there was an initial production of this mass fragment, the main decomposition happens in this range. The m/z = 29 fragment could be attributed to the +˙HC NH2 fragment of the chitosan ring. As the acetic acid evaporates during instrument equilibration time and does not show any characteristic MS peaks (Fig. S20, ESI†), the resemblance of the F/AA spectrum to that of pure chitosan is expected.
The TGA of the F/Tween sample shows a higher decomposition starting point (Tonset = 247 °C) compared to F/AA leading to significantly lower carbon residue (11 wt%) (Fig. S13, ESI†). It seems that the plasticiser has a double role, at lower temperatures it provides the film with thermal resistance, while at higher temperatures it promotes a cleaner burning of the film, leading to lower carbon residue.
The MS of F/Tween shows that the production of m/z = 29 is more apparent and also a product with m/z = 14 is released. The latter could be attributed to CH2+˙ released by the decomposition of Tween 80. The increase of m/z = 29 products could again be attributed to Tween, as CHO+˙ and C2H5+˙ fragments have identical masses. Also, around 450 °C a rapid production of atomic oxygen is observed, presumably due to the decomposition of Tween's side chains.
F/0.5LA shows a significantly lower decomposition point (Tonset = 167 °C) compared to F/AA (Fig. S14, ESI†). This can be explained by considering the presence of excess of lactic acid, which unlike acetic acid, remains physically bound to the film due to its lack of volatility. MS profile reveals the constant production of H2O throughout the temperature range, probably due to the initial decomposition of excess lactic acid. The TGA-MS spectrum of lactic acid (Fig. S21, ESI†) confirms the decomposition of the acid at a significantly lower temperature (Tonset = 145 °C). It is therefore possible that polymer-bound LA is released stepwise and decomposes over a larger temperature range.
TGA of F/bet:LA NaDES (Fig. S15, ESI†) is in general similar to bet:LA NaDES (Fig. S11, ESI†). The initial decomposition point has slightly shifted to higher temperature (Tonset = 201 °C) compared to the NaDES (192 °C). The carbon residue is almost doubled (from 3.6 to 6.5 wt%), due to the presence of chitosan. According to the synthetic procedure, a NaDES film consists of 83.3 wt% NaDES and 16.7% chitosan. Taking into account the carbon residue of bet:LA NaDES (3.4%) and F/AA (25.2%), as well as their relative ratios in the NaDES film, the theoretical carbon residue of the mixture is 6.8%, which is very close to the measured residue.
MS spectra of the thermal decomposition of the films show all the expected peaks of chitosan and lactic acid, accompanied with some extra peaks attributed to the presence of betaine. Peaks around 300 °C show that atomic and molecular oxygen are released, probably due to the decomposition of the carboxylic acid group. Another interesting peak is m/z = 40, which could be attributed to C–CH2–N+˙ due to the decomposition of betaine (Fig. S22, ESI†).
TGA-MS of F/bet:LA mix. (Fig. S16, ESI†) shows the same fragmentation pattern as F/bet:LA NaDES, without any major differences in the masses or the temperatures where they appear. TGA graphs, however, show some notable differences in the decomposition point (Tonset = 211 °C) and the carbon residue, which in this case is just 1%. These differences are indications that the structures of the films are actually different and the presence of the NaDES has an active role in the formation and structure of the film, compared to the simple addition of the individual components in solution.
Similar to the previous case, the TGA F/ChCl:LA NaDES (Fig. S17, ESI†) shows a significant shift in the decomposition point (Tonset = 225 °C) compared to ChCl:LA NaDES and F/AA. Specifically, this film shows the greatest resistance to thermal degradation of all the studied samples, as its decomposition point is higher than both individual components. The carbon residue is 5.1%, again almost identical to the theoretical carbon residue of the mixture (calculated 5%).
The MS spectra of the choline chloride containing films (F/ChCl:LA NaDES and F/ChCl:LA mix.) show the peaks for chitosan, with slight differentiations compared to F/bet:LA NaDES. In this case, oxygen release (m/z = 16 and 32) is insignificant, due to the presence of the hydroxyl group in choline chloride that decomposes in a different pathway compared to betaine. New peaks have appeared in this case, at m/z = 15, 50 and 52. These could be attributed to CH3+˙ and CH3Cl released from the decomposition of choline chloride. The relative ratio of m/z = 50 and 52 is exactly 76:24, which corresponds to the natural abundance of the two chlorine isotopes (35Cl and 37Cl). Thermal decomposition of ammonium chloride salts is widely studied and the nucleophilic elimination to alkyl chlorides is a generally accepted pathway.48,49
The TGA of F/ChCl:LA mix. (Fig. S18, ESI†) shows a lower decomposition point (Tonset = 209 °C) compared to F/ChCl:LA NaDES. More specifically, the decomposition point in this case is almost identical to that of the pure NaDES. The carbon residue follows the same trend as in the case of F/bet:LA NaDES, with the F/ChCl:LA mix. giving lower residue than expected (3.6 wt%) The MS fragmentation pattern is identical to F/ChCl:LA NaDES, with no noteworthy differences. Similarly, the TGA spectra of the betaine and choline chloride (Fig. S22 and S23 respectively, ESI†) indicate that the residue of betaine is higher than that of choline chloride.
Finally, as the water content is similar for the films containing the pre-formed NaDES or the corresponding mixture, it may be deduced that the slightly increased thickness observed in the former films (Table 2) is an inherent change, attributed to the polymer itself. A plausible explanation could be that the hydrogen bonding nature of the NADESs helps them permeate more between the chitosan chains, causing swelling of the polymer, which increases the volume of the film and, hence, its thickness.50
F/AA films present small holes with diameter of approximately 1.2 μm possibly due to the evaporation of the acetic acid. On the other hand, the F/Tween presents a very wrinkled structure without any pores or holes.
The two NaDES containing films (F/bet:LA NaDES and F/ChCl:LA NaDES) appear to have a very different morphology compared to the other films. Their surface appears to be smooth with small wrinkled structured pores. These pores appear to be more frequent and larger in the F/bet:LA NaDES compared to those of the F/ChCl:LA NaDES sample. The lactic acid containing film does not present any holes in its surface, possibly because lactic acid does not evaporate. Finally, the F/bet:LA mix. has a grain-like structure whereas the F/ChCl:LA mix. appears to have a wrinkled structured surface with pores.
SEM imaging revealed distinct differences among the films containing the NaDES or the corresponding mixture of the components. Comparing the F/bet:LA NaDES to the F/bet:LA mix. (Fig. 8c and f respectively), it can be observed that there is a uniformity in the surface of the former, while the latter has a less smooth surface. The same observation can be made when comparing the two choline chloride containing films.
The uniformity observed in the pre-formed NaDES containing films could be attributed to the existence some ‘clusters’ of the NaDES structure which, even though the dilution is high, are maintained probably due to the interaction with the chitosan macromolecule.
All reagents were used without further purification. In all experiments, MilliQ (18.2 MΩ at 25 °C) water was used.
The pH of aqueous solutions of the two NaDESs, as well as the pH of the solution of the physical mixtures of their components, was measured with a Metrohm 744 pH meter in order to identify the optimal concentration for the dissolution of chitosan (Fig. S1, ESI†). Chitosan can only be dissolved in acidic aqueous solutions where its primary amino groups are protonated and, as a result, the polymer becomes a positively charged polyelectrolyte.32 Typically, chitosan is dissolved in solutions of acetic acid, hydrochloric acid, formic acid or lactic acid. Therefore, concentration 1% w/v of the two NaDESs was selected as the pH was 3.
Film | Component concentration (aq. solution) | Component concentration (% w/v) | Plasticiser |
---|---|---|---|
F/AA | 1% v/v AA | 1.05% w/v | — |
F/Tween | 1% v/v AA | 1.05% w/v | 0.2% w/v Tween 80 |
F/bet:LA NaDES | 1% w/v bet:LA NaDES | 1.00% w/v | — |
F/bet:LA mix. | 1% w/v bet:LA mix. | 1.00% w/v | — |
F/0.5LA | 0.5% v/v LA | 0.61% w/v | — |
F/ChCl:LA NaDES | 1% w/v ChCl:LA NaDES | 1.00% w/v | — |
F/ChCl:LA mix. | 1% w/v ChCl:LA mix. | 1.00% w/v | — |
F/0.4LA | 0.4% v/v LA | 0.48% w/v | — |
WVP was calculated using the following equation:
W = (g/tA)·(x/ΔP) | (1) |
For each film, three repetitions of the measurement were performed.
Moisture content was calculated as the mass loss at T = 120 °C for all samples.
T onset: Temperature point where sample decomposition becomes significant. Calculated as the temperature point with 10% weight loss (after moisture loss).
T max.rate: Temperature of maximum decomposition rate.
T 1/2: Temperature of 50% sample mass loss (taking into account the carbonaceous residue).
Only little research on the field of chitosan dissolution directly into an aqueous solution of NaDES or their components42,51 has been conducted and should be investigated further, as the low solubility of the polymer in a number of common solvents constitutes a major drawback. Our work was mainly focused on the preparation of the films and the comparison of their properties, therefore the full capacity of NaDESs’ capability of dissolving chitosan is an aspect worthy of future investigation.
The obtained results suggest that the properties of the films can be easily adjusted to fit the requirements of a wide range of applications. The NaDES containing films or the films containing the physical mixture of the corresponding NaDES are very elastic and allow water to easily pass through. On the other hand, the films that do not contain a NaDES were inelastic and very resistant to rupture.
Additionally, the selection of NaDES also plays a vital role on the final properties of the films. The betaine containing films were twice as elastic as the choline chloride containing films, while the permeation of water through was only half. The presence of chitosan slightly affects the thermal properties of the films, increasing the indicative temperatures Tonset, Tmax.rate and T1/2. SEM imaging revealed that the addition of a pre-formed NaDES, offers a uniformity on the morphology of the film, whereas, the separate addition of the two components is responsible for an uneven surface.
Our study indicates that the NaDES films are not completely identical to those produced from the direct mixture of NaDES's components. Indeed, the films appear to have almost identical DB and BS values, while the WVP, FTIR and thermal analysis reveal some minor differences. The mixture-films appear to be slightly better water vapour barriers and to decompose at slightly higher temperatures compared to the NaDES-films. Moreover, the FTIR of the produced films also appear to be non-identical. These results are consistent in our study, as they agree in both NaDES cases and are observed over multiple repetitions of our experiments. The observed differences are small, but statistically significant, and do not match our initial theory that the films should be completely identical regardless the production method. Therefore, further studies need to be conducted in order to completely understand the interactions in DES and how they are affected when they are diluted.
The aforementioned results demonstrate that the chitosan-stabilised NaDES films are very promising alternatives for biomedical applications. Commercial wound healing patches and wound closure strips are mostly made of synthetic rubber enriched with bioactive compounds to promote healing, but usually lack in terms of elasticity. The prepared films are highly elastic, which allows the material to stretch with the skin's movements, which is significant for a safe and scar-free healing. On the other hand, the NaDESs used could be extracted and reused, leaving a porous material, consisting of pure chitosan with antibacterial properties.52 Moreover, the sustainable and biodegradable character of the product is of upmost importance for the reduction of health-care waste, which according the World Health Organisation has risen to approximately 1900 tonnes per year.53
Footnote |
† Electronic supplementary information (ESI) available: pH curves of the NaDESs aqueous solutions, FT-IR spectra and TGA graphs of the NaDESs, deconvoluted FT-IR spectra of the films, TGA-MS of the films and the starting materials. See DOI: 10.1039/d0ma01008a |
This journal is © The Royal Society of Chemistry 2021 |