Yasuyuki
Yamada
*ab,
Yusuke
Miwa
a,
Yuka
Toyoda
b,
Quan Manh
Phung
ac,
Kin-ichi
Oyama
b and
Kentaro
Tanaka
*a
aDepartment of Chemistry, Graduate School of Science, Nagoya University, Furo-cho, Chikusa-ku, Nagoya 464-8602, Japan. E-mail: kentaro@chem.nagoya-u.ac.jp; yy@chem.nagoya-u.ac.jp
bResearch Center for Materials Science, Nagoya University, Furo-cho, Chikusa-ku, Nagoya 464-8602, Japan
cInstitute of Transformative Bio-Molecules (ITbM), Nagoya University, Furo-cho, Chikusa-ku, Nagoya 464-8601, Japan
First published on 31st January 2023
A μ-nitrido-bridged dimer of iron phthalocyanine is one of the most potent molecule-based CH4 oxidation catalysts reported to date. The reactive intermediate is a high-valent iron-oxo species generated through reaction with H2O2 in an acidic aqueous solution. However, there are few reports on the synthesis and catalytic CH4 oxidation activity of a μ-nitrido-bridged heterodimer of two different iron porphyrinoids, despite that there are a variety of iron porphyrinoids with coordination and electronic structures different from those of iron phthalocyanines or iron porphyrins. Herein, we report the synthesis of a novel μ-nitrido-bridged heterodimer of an iron phthalocyanine and iron porphycene and examine its CH4 oxidation activity. Porphycenes are an important class of porphyrinoids with a smaller coordination sphere than phthalocyanines or porphyrins. Single crystal structural analyses revealed that the heterodimer possessed a Fe–N
Fe core structure similar to that of the phthalocyanine homodimer. The heterodimer showed catalytic CH4 oxidation activity in an acidic aqueous solution in the presence of H2O2 at 60 °C through the high-valent iron-oxo species as in the case with the phthalocyanine homodimer. This was in clear contrast to the result that the high-valent iron-oxo species of a μ-nitrido-bridged iron porphycene dimer was so unstable that it decomposed quickly in the same reaction conditions.
However, from the viewpoint of catalytic activity, a very limited number of artificial molecular iron-oxo-based biomimetic catalysts exist that activate the C–H bonding of CH4 at temperatures lower than 100 °C because of the high stability of CH4.3,18,20 A. B. Sorokin et al. found that a μ-nitrido-bridged iron phthalocyanine (Pc) dimer (1 or 1+) reacts with H2O2 in an acidic aqueous solution to afford a high-valent iron-oxo species 1oxo, which shows a particularly high CH4 oxidation activity among various molecular CH4 oxidation catalysts at a lower temperature than 100 °C (Fig. 1a).20–22 Similarly, μ-nitrido-bridged iron porphyrin dimer 2 was reported to indicate CH4 oxidation activity comparable to that of μ-nitrido-bridged iron phthalocyanine dimer (Fig. 1b).23 According to some theoretical estimates, the core μ-nitrido-bridged dinuclear iron structure (Fe–N
Fe) is believed to be crucial in the reaction of these high CH4 oxidation activities.24–27
Inspired by these previous works, we recently synthesized μ-nitrido-bridged dinuclear iron porphycene (Ppc) dimer 3+, a structural analog of 1+, and investigated its CH4 oxidation activity (Fig. 1c).28 Porphycene is an important class of porphyrinoids and has a rectangular-shaped narrower cavity than phthalocyanine, which renders the coordination structures and reactivities of the metal complexes different from those of phthalocyanine.29,30
Although 3+ has a μ-nitrido-bridged dinuclear iron core (Fe–N
Fe) similar to that of 1+, it was found that 3+ showed less CH4 oxidation activity, and the reaction proceeded through a different mechanism (Fenton-type reaction; the reaction intermediate is ˙OH). This is presumably because the high-valent iron-oxo species 3oxo is less stable than 1oxo and decomposes during the CH4 oxidation reaction. The decomposed product could act as a catalyst for ˙OH production. These results indicate that the difference in the structure of the porphyrinoid moiety strongly affects the reactivity of the high-valent iron-oxo species.
In this study, we report the synthesis of a μ-nitrido-bridged heterodimer of an iron phthalocyanine and an iron porphycene (4+, Fig. 1d) and its CH4 oxidation activity. Thus far, there have been very few reports investigating the CH4 oxidation activity of μ-nitrido-bridged heterodimers of iron porphyrinoids. We previously confirmed that a supramolecular μ-nitrido-bridged heterodimer of an iron porphyrin and an iron phthalocyanine provided sufficiently stable high-valent iron-oxo species for catalytic CH4 or CH3CH3 oxidation reactions.31,32 It has also been reported that H2O2 preferentially reacts with the electron-rich iron phthalocyanine moiety of the μ-nitrido-bridged heterodimer of an electron-rich iron phthalocyanine and an electron-deficient iron phthalocyanine to afford a high-valent iron-oxo species, although the reactivity of the heterodimer has not been reported.33 Therefore, the fact that a μ-nitrido-bridged iron phthalocyanine dimer 1 (or 1+) indicated potent CH4 oxidation activity through the reaction of high-valent iron-oxo species, whereas a μ-nitrido-bridged dinuclear iron porphycene dimer 3+ showed a different CH4 oxidation mechanism, prompted us to clarify the relationship between the structure and reactivity of 4+.
:
1 mixture of iron porphycene 5 and iron phthalocyanine 6 with NaN3 improved the isolated yield of 4+·I3− to 71%. Elemental analysis suggested that the counter anion of the monocationic heterodimer was triiodide, which was further confirmed using single-crystal X-ray structural analysis.
![]() | ||
| Fig. 2 (a) Synthesis of a monocationic heterodimer 4+·I3−. (b) 1H-NMR spectrum of 4+·I3− in pyridine-d5. | ||
1H-NMR and MALDI-TOF MS analyses were performed to characterize 4+·I3−. In the MALDI-TOF MS spectrum shown in Fig. S1 in the ESI,† a signal corresponding to 4+ was observed at m/z = 1250.26, which corresponds to the theoretical isotope distribution pattern of 4+. As shown in Fig. 2b, all the 1H-NMR peaks of 4+·I3− were observed as sharp signals in the range of 6–10 ppm. A neutral μ-nitrido-bridged FeTPP dimer containing Fe(III) and Fe(IV) was reported to indicate a significant broadening of the 1H-NMR signals, whereas its monocationic species containing two Fe(IV) centers showed sharp 1H-NMR signals because the two Fe(IV) centers interacted with each other in an antiferromagnetic manner.34–36 Therefore, it is considered that 4+·I3− includes two Fe(IV) ions interacting with each other in an antiferromagnetic manner. Moreover, considering that two sets of signals corresponding to those of the o- and m-protons of the peripheral phenyl groups were observed, the rotation of the peripheral phenyl groups of the porphycene ring was restricted owing to steric repulsion between the phenyl groups and the porphycene ring, as in the case of the previously reported μ-nitrido-bridged dinuclear iron porphycene dimer 3+·PF6−. However, the rotation of the porphycene ring along the Fe–N
Fe axis was sufficiently fast compared to the NMR timescale because the porphycene ring was observed as a C2 symmetrical structure.
A comparison of the UV-vis spectrum of 4+·PF6− with those of μ-nitrido-bridged iron phthalocyanine dimer 1+·I− and μ-nitrido-bridged iron porphycene dimer 3+·PF6− is shown in Fig. 3. The bands at 357 and 399 nm were assignable to the absorptions by the phthalocyanine and porphycene units, respectively, both of which showed significant shifts compared to those of the homoleptic dimers 1+·I− and 3+·PF6−.28,37 The Q-band of the phthalocyanine unit of 4+·PF6− at 634 nm showed an apparent hypochromic shift compared to that of the phthalocyanine dimer 1+·I−, whereas the Q-band of the phthalocyanine unit of 4+·PF6− at 705 nm appeared at a higher wavelength than that of 1+·I−. These results implied an apparent electronic interaction between the two porphyrinoids in 4+·PF6−.
![]() | ||
| Fig. 3 Comparison of UV-vis spectra of a heterodimer 4+·PF6− and two homodimers, 1+·I− and 3+·PF6−, in pyridine at 20 °C. | ||
:
1 (v/v) mixture of pyridine and CHCl3. The molecular structures of 4+·I3− are shown in Fig. 4a and b.
![]() | ||
| Fig. 4 (a) Side and (b) top views of the single crystal X-ray structure of 4+·I3−. I3−, coordinating pyridines, and crystalline solvents were omitted for clarity. (c) Comparison of some mean bond lengths and angles of 4+·I3−, 1+·I−, and 3+·PF6−. *1: ref. 28, *2: ref. 38. | ||
The distance between the μ-nitrogen and Fe(IV) ion in porphycene (1.62(9) Å) is almost identical to that of the μ-nitrogen and Fe(IV) ion in phthalocyanine (1.66(4) Å), suggesting that the Fe–μ-N–Fe core has a π-conjugated structure. The mean bond distances between the four porphycene nitrogens and the coordinated Fe(IV) ion (1.93 Å) are almost identical to those between the four phthalocyanine nitrogens and the coordinated Fe(IV) ion (1.94 Å). The average bond angles of the μ-nitrogen–Fe–nitrogens(porphyrinoid) in 4+·I3− were 93.45(8)° for iron phthalocyanine and 93.13(3)° for iron porphycene, both of which were slightly larger than 90°. The core-coordinating N4 planes of the two porphyrinoid rings are located in an almost parallel configuration. The phthalocyanine ring was slightly distorted from the planar structure, presumably because of steric repulsion between the phthalocyanine ring and peripheral phenyl groups of the porphycene ring. As suggested by 1H NMR spectroscopy, the rotation of the peripheral phenyl groups of the porphycene ring appeared to be significantly suppressed by steric repulsion between the phenyl groups and porphycene rings.
A comparison of the single-crystal structure of 4+·I3− with those of 1+·I− and 3+·PF6− is summarized in a table shown in Fig. 4c.28,38 Although slight differences were observed in the distance between nitrogen and Fe(IV) and the average bond angles of the μ-nitrogen–Fe–nitrogen (porphyrinoid), these differences are presumably derived from the heteroleptic structure of 4+·I3−. Overall, it could be concluded that 4+·I3− has a similar Fe–N–Fe core structure to those of 1+·I− and 3+·PF6−. The relative angle between the phthalocyanine ring and the long axis of the porphycene ring was calculated to be 17.4°, which was much smaller than the relative angles between the two porphyrinoid rings in 1+·I− (37.5°) and 3+·PF6− (42.2°). We attributed this difference in the relative angle between the two porphyrinoids to the difference in the packing structure, because both rings in 4+·I3− are rotatable along the Fe–N
Fe axis.
In the case of a voltammogram of a μ-nitrido-bridged iron phthalocyanine dimer 1+·I− (shown in Fig. 5b), Ercolani et al. carefully investigated the redox processes to conclude that the four redox waves at −0.58, −1.52, −1.74 and −2.00 V should be assignable to the redox in the iron cores of 1+·I−.39 For the voltammogram of a μ-nitrido-bridged iron porphycene dimer 3+·PF6− shown in Fig. 5c, we assigned the 1st (−0.90 V vs. Fc+/Fc), 2nd (−1.32 V), 3rd (−1.49 V), and 4th (−1.78 V) reduction waves of the porphycene dimer to those of Fe(IV)Fe(IV)/Fe(III)Fe(IV), Fe(III)Fe(IV)/Fe(III)Fe(III), Fe(III)Fe(III)/Fe(II)Fe(III), and Fe(II)Fe(III)/Fe(II)Fe(II), respectively. This is based on the fact that Gross et al. investigated the detailed redox properties of a 2,7,12,17-tetra-n-propylporphycene iron(III) chloride (ClFeTprPpc), a monomeric porphycene, by electrochemical and spectroelectrochemical measurements to report that the reduction of the iron center (Fe(III)/Fe(II)) occurred at more positive potential than that of the porphycene center (TPrPpc/TPrPpc˙−).40 Similarly, it is assumed that at least the four reduction waves of 4+·PF6− at −0.75, −1.37, −1.69, and −1.92 V could be assignable to those of the iron centers of 4+·PF6−. Thus, it was demonstrated that 4+·PF6− has a completely different electronic structure from those of 1+·I− and 3+·PF6− owing to the different types of porphyrinoid rings.38
As for the oxidation of 4+·PF6−, theoretical calculations suggested that the phthalocyanine ring is more easily oxidized than the porphycene ring (vide infra, see “DFT calculations” section). In addition, the μ-nitrido-bridged iron phthalocyanine dimer 1+·I− showed a lower oxidation potential at −0.19 V than that of a μ-nitrido-bridged iron porphycene dimer 3+·PF6− at 0.68 V, both of which are assignable to the oxidations of the porphyrinoid cores. Therefore, the oxidation wave at 0.50 V is assignable to that of the phthalocyanine ring. Overall, 4+·PF6− showed a first reduction wave higher than that of 1+·I− and lower than that of 3+·PF6−, whereas the first oxidation wave of 4+·PF6− was observed at potentials higher than 1+·I− and lower than 3+·PF6−.
As shown in Fig. 6, the signals assignable to those of the high-valent iron-oxo species ([4 + O]+) were observed at approximately m/z = 1266 after the addition of aqueous H2O2 at room temperature, with its isotopic distribution pattern corresponding to that of the calculated pattern. The signals observed at approximately 1284 correspond to those of the hydroperoxo species ([4 + HOOH]+). We also confirmed that treatment of 4+·I3− with H218O2 resulted in the generation of the peaks assignable to [4 + 18O] as shown in the ESI.† These results demonstrate that high-valent iron-oxo species were generated after the threat of 4+ with H2O2via the corresponding hydroperoxo species, as in the case with the other μ-nitrido-bridged iron phthalocyanine dimers. Sorokin et al. reported that treatment of heteroleptic μ-nitrido-bridged dimer of iron phthalocyanine and iron porphyrazine with m-chloroperbenzoic acid (mCPBA) resulted in the attachment of oxo moiety either on the iron phthalocyanine and iron porphyrazine. In this case, they concluded that the attachment of oxo moiety occurred with slight preference for the iron phthalocyanine unit based on the results of cryospray collision induced dissociation MS/MS technique.41 However, in the case ESI-TOF MS analysis of [4 + O]+, it was difficult to determine the accurate position of the Fe
O moiety (whether it is on the iron porphycene or the iron phthalocyanine in 4+) even after MS/MS analysis of the [4 + O]+ peak because the ionization efficiency of the Fe-phthalocyanine fragments was much smaller than that of the Fe-porphycene fragments.
Upon reduction, both Fe–N(μ) bonds were lengthened as an antibonding orbital comprising Fe(3dz2) and N(2s) orbitals. The difference between the two Fe–N(μ) bonds is only 0.03 Å, indicating that the two Fe centers are similar and the complex could be formally characterized as Fe3.5–N–Fe3.5.20 Spin populations also reveal that both Fe centers are involved in the reduction, with Fe(Pc) being slightly more reduced than Fe(Ppc). Upon oxidation, the Fe–N(μ) bond lengths change by less than 0.01 Å, indicating that the oxidation occurs mainly at the macrocycles. The spin population of Pc is 0.76, whereas Ppc has a spin population of 0.15. This difference in the spin density implies that oxidation primarily occurs at Pc. The higher tendency of phthalocyanine to be oxidized is related to its longer conjugation length compared to that of porphycene.
We now compare the two oxo isomers, O
Fe(Pc)–N–Fe(Ppc) and O
Fe(Ppc)–N–Fe(Pc) (DFT structures are shown in Fig. 7). Similar to a previous work,27 two doublet states were calculated: the ground state in which one of the macrocycles was oxidized FeIVFeIV(P˙+) and a low-lying excited state FeIVFeV (Fig. S4†). Selected bond lengths are listed in Table S3.† The Fe–N–Fe fragment is no longer symmetric. The general trend is that the formation of Fe-oxo significantly increases the length of the adjacent Fe–N(μ) bond above 1.7 Å. DFT predicts that O
Fe(Pc)–N–Fe(Ppc) and O
Fe(Ppc)–N–Fe(Pc) are close in energy. The former isomer (in pyridine at 298 K) was slightly more stable (2–4 kcal mol−1) than the latter (Table S5†).
Considering that the phthalocyanine ring is more easily oxidized than the porphycene ring, H2O2 might coordinate to Fe-porphycene more strongly than to Fe-phthalocyanine because the porphycene ring is more electron deficient than the phthalocyanine ring. This suggests that the oxo species of 4+ could be preferentially generated on the Fe-porphycene moiety. This prompted us to compare the stability of the hydroperoxo species on the Fe-porphycene ring (HOOFePpc–N
FePc) with that of the Fe-phthalocyanine ring (HOOFePc–N
FePpc). We found that the difference between these two species is quite small (ca. 3 kcal mol−1; HOOFePpc–N
FePc is more stable than HOOFePc–N
FePpc). Moreover, we compared the O–O bond dissociation free energy in HOOFePpc–N
FePc and HOOFePc–N
FePpc because dissociation of the O–O bond is indispensable for the generation of iron-oxo species from hydroperoxo species. However, it was demonstrated that both hydroperoxo species have similar O–O bond dissociation free energy (37.2 kcal mol−1 for HOOFePpc–N
FePc and 36.7 kcal mol−1 for HOOFePc–N
FePpc in pyridine).
Considering the uncertainty in DFT calculations, the results obtained from DFT calculation propose that both oxo isomers (O
Fe(Pc)–N–Fe(Ppc) and O
Fe(Ppc)–N–Fe(Pc)) could be produced. However, it is also important to consider that the formation of oxo isomers should be kinetically controlled. The complete reaction mechanisms for the production of high-valent iron-oxo species are outside the scope of this study.
To appropriately evaluate the catalytic CH4 oxidation activity, the effective total turnover number (TTNeff) and effective methane conversion number (MCNeff) were defined according to eqn (i)–(iv), based on the idea that CH4 is oxidized in a stepwise manner, as shown in Fig. 8b.
| TTNeff = TTN(CH4) − TTN(N2) | (i) |
| TTN(CH4) or TTN(N2) = (CMeOH + 2 × CHCHO + 3 × CHCOOH)/CCat | (ii) |
| MCNeff = MCN(CH4) − MCN(N2) | (iii) |
| MCN(CH4) or MCN(N2) = (CMeOH + CHCHO + CHCOOH)/CCat | (iv) |
Fig. 9a shows the time dependence of TTNeff. Although TTNeff increased almost linearly at the initial stage, the rate of increase increased, particularly after 32 h of oxidation. It should also be mentioned that the bluish-green color of the catalyst apparently became thinner, especially after 32 h, and almost colorless after 48 h of oxidation (Fig. S5†), suggesting that the porphyrinoid core of 4+·I3− gradually decomposed during the reaction. A similar bleaching of the color of the catalyst was observed in the oxidation reaction using the porphycene dimer 3+·PF6−. However, the bleaching speed was much slower for 4+·I3−, implying that the stability of 4+·I3− is higher than that of 3+·PF6− under these reaction conditions. Considering that apparent bleaching was not observed in the case of the phthalocyanine dimer 1+·I−, the higher stability of 4+·I3− than 3+·PF6− might be because the phthalocyanine unit in 4+·I3− contributed to the stable generation of the high-valent iron-oxo species after the reaction with H2O2.
To further investigate the reaction mechanism of CH4 oxidation by 4+·I3−, we performed the CH4 oxidation in the presence of Na2SO3, a radical scavenger (Fig. 9a and Table S7,† entries 6 and 7).44 It was demonstrated that the reaction after 24 h of oxidation was suppressed by approximately 63%, whereas the reaction after 48 h of oxidation was suppressed to 50%. This indicates that the oxidation reaction mainly proceeded through the high-valent iron-oxo species, at least in its initial stage. However, considering that the color of 4+·I3− gradually bleached, particularly after 32 h, oxidation by the Fenton-type reaction via ˙OH gradually increased, presumably because the decomposed product acted as the catalyst for the Fenton-type reaction, as summarized in Fig. 9b. Because ˙OH is so reactive that it can even decompose the porphyrinoid cores of 4+·I3−, the accelerated decomposition of the catalyst is not only because of the intrinsic instability of the catalyst, but also because of the decomposition by ˙OH.
Fig. 9c shows a comparison of TTNeff and MCNeff of 1+·I−, 3+·PF6−, and 4+·I3− after 24 h of oxidation under the same reaction conditions. The reason why 4+·I3− showed less CH4 oxidation activity than the porphycene dimer 3+·PF6− is that 3+·PF6− decomposed more rapidly and CH4 oxidation for 24 h mostly proceeded via a Fenton-type reaction. However, both TTNeff and MCNeff for oxidation by 4+·I3− were much less than in the case of oxidation by 1+·I−, which mostly proceeded via the high-valent iron-oxo species. Therefore, it can be concluded that the catalytic methane oxidation activity via the high-valent iron-oxo species of 4+·I3− (O
FePpc–N
FePc and/or O
FePc–N
FePpc) is lower than that of the high-valent iron-oxo species of 1+·I− (O
FePc–N
FePc). This result indicates that the reactivity of the μ-nitrido-bridged iron porphyrinoid dimer strongly reflects the difference in the porphyrinoid skeleton, although the structures of the Fe–N
Fe cores are quite similar. We consider that one possible explanation for the lower catalytic activity of 4+·I3− than 1+·I− could be the slow generation of the high-valent iron-oxo species of 4+·I3− than that of 1+·I− because of the lower efficiency of the push effect, which facilitates the heterolytic O–O bond cleavage of the hydroperoxo species (Fe–O–OH) owing to the lower electron-donating ability of the porphyrinoid ring of 4+, as can be estimated from the fact that the oxidation potential of the phthalocyanine ring of 4+·I3− is higher than that of 1+·I−.
Fe core structure of 4+·I3− is similar to that of a monocationic μ-nitrido-bridged iron phthalocyanine dimer (1+·I−) and a monocationic μ-nitrido-bridged iron porphycene dimer (3+·PF6−). ESI-TOF MS study indicated that treatment of 4+·I3− with H2O2 gave the high-valent iron-oxo species of 4+. DFT calculations suggested that the high-valent iron-oxo species of 4+·I3− could be generated on both iron-porphycene and iron-phthalocyanine rings through the reaction with H2O2. The catalytic CH4 oxidation reaction by 4+·I3− in an acidic aqueous solution proceeded in the presence of excess H2O2 to afford a mixture of MeOH, HCHO, and HCOOH through the high-valent iron-oxo species at its initial stage as in the case with 1+·I−. It was demonstrated that the catalytic activity of the high-valent iron-oxo species of 1+·I− was higher than that of 4+·I3−. However, as the reaction time was elongated, it was found that 4+·I3− was gradually decomposed. This implies that the high-valent iron-oxo species of 4+·I3− was less stable than that of 1+·I−. Considering that the high-valent iron-oxo species of 3+·PF6− is much less stable and readily decomposes under the same reaction conditions, the lower stability of the high-valent iron-oxo species of 4+·I3− compared to that of 1+·I− is derived from the difference in the porphyrinoid ring. Thus, it was confirmed that the difference in the porphyrinoid ring of the monocationic μ-nitrido-bridged iron porphyrinoid dimer strongly affected the stability of the high-valent iron-oxo species as well as the catalytic activity of the monocationic μ-nitrido-bridged iron porphyrinoid dimer. We believe that these findings would provide some valuable insights for the future development of molecular CH4 oxidation catalysts based on μ-nitrido-bridged iron porphyrinoid dimers.
:
1 (v/v) mixture of pyridine and CHCl3. Single-crystal X-ray diffraction measurements were performed using a Rigaku X-ray diffractometer equipped with a molybdenum MicroMax-007 and Saturn 70 CCD detector. The measurement was performed at 123 K. The structure was solved via the direct method (SHELXT) and refined via full-matrix least-squares on F2 (SHELX-2018) using Olex2-1.3 program. All non-hydrogen atoms were refined anisotropically. Geometrical restraints were applied: DFIX, SADI, SIMU, ISOR, and OMIT. The crystal data are as follows: formula C74H49.6Cl15.6Fe1.6I2.4N12, FW = 2053.882, crystal size 0.19 × 0.20 × 0.22 mm3, triclinic, space group P
, a = 20.6469(2) Å, b = 23.6627(3) Å, c = 24.8965(3) Å, α = 64.380(1)°, β = 69.270(1)°, γ = 68.880(1)°, V = 9942.9(2) Å3, Z = 5, R1 = 0.1207 (I > 2(I)), wR2 = 0.3227 (all), GOF = 1.110. CCDC identification code 2217367. All the checkCIF Level-B alerts are due to the low crystal quality.
:
1 (v/v)). After the addition of silica gel (1082 mg) to the solution, solvent was evaporated. CHCl3 (10 mL) was added to the residue. After solvent was evaporated, the residue was dried under vacuum at 60 °C over night. The catalyst was suspended in an aqueous TFA (TFA 10.0 mL + H2O 100 mL). The mixture was sonicated for 30 min and then the solid was filtered. This TFA wash procedure was repeated twice. Finally, the resulting solid was washed with H2O (300 mL) and dried under vacuum at 60 °C over night. The silica-supported catalyst was obtained quantitatively.
Footnote |
| † Electronic supplementary information (ESI) available. CCDC 2217367. For ESI and crystallographic data in CIF or other electronic format see DOI: https://doi.org/10.1039/d2cy01980a |