aFriedrich-Alexander-Universität Erlangen-Nürnberg (FAU), Lehrstuhl für Chemische Reaktionstechnik (CRT), Egerlandstraße 3, 91058 Erlangen, Germany. E-mail: marco.haumann@fau.de; peter.wasserscheid@fau.de
bFriedrich-Alexander-Universität Erlangen-Nürnberg (FAU), Lehrstuhl für Feststoff- und Grenzflächenverfahrenstechnik (LFG), Cauerstraße 4, 91058 Erlangen, Germany
cResearch Centre for Synthesis and Catalysis, Department of Chemistry, University of Johannesburg, P.O. Box 524, Auckland Park 2006, South Africa
dForschungszentrum Jülich GmbH, Helmholtz-Institute Erlangen-Nürnberg for Renewable Energy (IEK 11), Egerlandstraße 3, 91058 Erlangen, Germany
First published on 10th July 2023
Supported catalytically active liquid metal solution (SCALMS) materials represent a recently developed class of heterogeneous catalysts, where the catalytic reaction takes place at the highly dynamic interface of supported liquid alloys. Ga nuggets were dispersed into nano-droplets in propan-2-ol using ultrasonication followed by the addition of Pt in a galvanic displacement reaction – either directly into the Ga/propan-2-ol dispersion (in situ) or consecutively onto the supported Ga droplets (ex situ). The in situ galvanic displacement reaction between Ga and Pt was studied in three different reaction media, namely propan-2-ol, water, and 20 vol% water containing propan-2-ol. TEM investigations reveal that the Ga–Pt reaction in propan-2-ol resulted in the formation of Pt aggregates on top of Ga nano-droplets. In the water/propan-2-ol mixture, the desired incorporation of Pt into the Ga matrix was achieved. The ex situ prepared Ga–Pt SCALMS were tested in n-heptane dehydrogenation. Ga–Pt SCALMS synthesized in pure alcoholic solution showed equal dehydrogenation and cracking activity. Ga–Pt SCALMS prepared in pure water, in contrast, showed mainly cracking activity due to oxidation of Ga droplets. The Ga–Pt SCALMS material prepared in water/propan-2-ol resulted in high activity, n-heptene selectivity of 63%, and only low cracking tendency. This can be attributed to the supported liquid Ga–Pt alloy where Pt atoms are present in the liquid Ga matrix at the highly dynamic catalytic interface.
The first generation of Ga-based SCALMS catalysts was synthesized via an organometallic route that involved (Et3N)GaH3 as volatile Ga precursor (see Fig. 1c). However, (Et3N)GaH3 is very air-sensitive and hence its synthesis and handling require strictly inert conditions. Additionally, since large excess of LiH is required for the synthesis, the process produces a significant amount of noxious waste, hampering the scalability of this SCALMS preparation route.15 Typically, less than 5% of the atoms in the starting materials show up in the final catalyst (see ESI† for details). Therefore, an alternative top-down synthetic procedure has been introduced recently.8 This scalable approach includes only two process steps: in the first step, elemental Ga is dispersed into micro- and nano-droplets in propan-2-ol using ultrasonication, creating a stable Ga/propan-2-ol dispersion. In the second step, the catalytically active metal is introduced into the elemental Ga droplets via galvanic displacement (see Fig. 1c). Conversely to the previously applied precursor route using (Et3N)GaH3, the synthesis of SCALMS via the top-down sonification route produces no waste and is characterized by nearly 100% atom efficiency.8
Ultrasonication is widely used to reduce the droplet size of liquid metals such as Ga (ref. 8, 16 and 17) and its eutectic mixtures, such as GaIn (ref. 18–22) and GaInSn (ref. 23) (see Table S1† for details). The average particle size formed during ultrasonication depends on the geometry of the sonication vessel, total power input, sonication amplitude, duration, and temperature as well as on the physicochemical properties of the continuous phase.17,24 It has been reported that by using ethanol or propan-2-ol as continuous phase under ambient conditions, a high yield of Ga nano-droplets is obtained, without the need for stabilizers or surfactants.18,19,25 The exact reason for the Ga droplet stability is not clear. It is supposed that the formation of a Ga2O3 passivation skin and/or the formation of a carbon layer coating the surface of the Ga nano-droplets provides stabilization.22,23,26 However, recent work by Creighton et al.19 supports the conclusion of a dominant stabilization by a Ga2O3 passivation layer. These authors showed that working under ambient atmosphere Ga droplets with a mean particle size of ∼150 nm are produced while identical conditions in an oxygen-free and moisture-free atmosphere resulted in the formation of much larger Ga droplets in the range of 1 to 2 μm.19
The introduction of precious metals into a Ga matrix can be carried out using the galvanic displacement reaction (GDR). GDR represents a simple and versatile method to synthesize tailored bimetallic nanostructures. The method offers control over composition, size, shape, and internal structure.27–31 GDR is a redox process, in which a metal is replaced by the ions of a second metal when they come into contact in a solution phase. In principle, the GDR should occur spontaneously between any two metals with a favorable driving force, i.e., a suitable difference in their reduction potentials.27 The morphology of bimetallic nanoparticles or nano-droplets obtained by GDR is affected by the reactivity of the metals involved, the concertation of metallic ions, and the reaction temperature.27,32 Since GDR depends on the difference in reduction potentials of the metals (determined under standard conditions), the involvement of non-standard conditions can affect the actual reduction potential. This can slow down, reverse, or even prevent the replacement reaction.27 Even though the majority of applications are limited to “solid” metallic nanoparticles, recently this elegant approach was extended to “liquid” metal alloy such as galinstan and its reaction with Pt,28 Ag,29,32 Au,29,32 Cu,30,32 and Sn (ref. 32) to form bimetallic nanoparticles. More recently, the chemical reactivity of liquid gallium in galvanic displacement reaction with Cu,33–35 Ni,33 Sn,33 and Cd (ref. 33) was explored. However, to the best of our knowledge, the factors affecting the galvanic displacement reaction between liquid gallium droplets and Pt ions have not been studied yet, which is somewhat surprising given the high relevance of supported Ga–Pt droplets for catalytic applications.8,9
If Ga-based SCALMS materials are handled in contact with air, the Ga droplets are normally surrounded by a thin Ga2O3 passivation layer. Even though metallic gallium is inert for C–H bond activation,6 Ga2O3 is a known catalyst for alkane dehydrogenation reactions36–38 but shows fast deactivation behavior.38 Additionally, Ga2O3 is an amphoteric oxide and has been found to act as a bifunctional catalyst, e.g., to promote the conversion of alkanes to aromatics via heterolytic dissociation over Lewis acid/base pairs37,39 or for the cracking of longer alkanes to lighter ones.39–41 For the direct dehydrogenation of alkanes to n-alkenes, however, a clean noble metal surface is beneficial.2 Hence, the conversion of alkanes to n-alkenes can be regarded as a good test reaction to find out whether a given catalyst material acts as a cracking, cyclization, isomerization, or as a dehydrogenation catalyst depending on the nature of its active sites.42 While noble metals, such as Pt, are well known to activate or recombine H2, metal oxides such as Ga2O3 can promote acid-catalyzed isomerization and cyclization reactions.42,43 The concerted action of both noble metal sites and acid sites enables hydrocracking, hydroisomerization, dehydrocyclization, and aromatization reactions. Since Ga2O3-rich catalysts are less selective in direct n-alkane dehydrogenation the reductive removal of this oxide skin (e.g., by pre-formation with hydrogen) has been found crucial to reaching high n-alkene selectivities.36,39,44
In Ga-based SCALMS, the thickness of the Ga2O3 passivation layer on the supported Ga droplets depends on the synthetic protocol and the synthesis conditions (i.e., moisture content of the applied solvents, calcination temperature, etc.). Fortunately, the Ga2O3 layer can be reduced to Ga0 under a reductive atmosphere in the presence of noble metals such as Pt.36 Hydrogen pre-treatment at elevated temperatures is thus able to remove the Ga2O3 skin before reaction. However, if the Ga2O3 layer becomes too thick the reduction of the oxide layer may not be complete and the resulting presence of some leftover Ga2O3 can lead to side reactions.
It has also been reported that Ga2O3 can form mixed oxides with oxidic supports, such as Al2O3, and that the resulting mixed oxide is more difficult to reduce.36,45–47 Therefore, it is important to keep the oxidation of the Ga droplet surface to a minimum during the SCALMS preparation to enable catalysis with reduced supported Ga–Pt droplets after reductive catalyst activation.
In this contribution, we present a detailed investigation of the synthesis of Ga nano-droplets using ultrasonication. In addition, we study the effect of the reaction medium on GDR between Ga and Pt as well as on the morphology of the Ga–Pt nanocomposites formed. Finally, we investigate the effect of these catalyst material synthesis parameters on the resulting catalytic performance in n-heptane dehydrogenation.
To monitor the depletion of Pt concentration from the continuous phase of the dispersion, aliquots of 2 mL were taken every 2 minutes using a syringe and immediately filtered using a 0.1 μm syringe filter to remove Ga droplets. The syringe filter was then washed 3 times with 3 mL propan-2-ol or water. This filtered solution was analyzed for its Pt content using ICP-AES to monitor the remaining Pt in the solution. From this, the depletion of Pt from the continuous phase was calculated, which corresponds to the amount of Pt reacted with Ga.
(1) |
All SCALMS materials were dried after preparation under vacuum at 313 K using a rotary evaporator. The resulting materials were then calcined for 2 hours at 773 K under ambient conditions. The final loading of Ga and Pt was verified by ICP-AES.
For in situ preparation of Ga–Pt SCALMS-C*, the GDR was carried out directly in the Ga-dispersion in a water/propan-2-ol mixture (see Fig. 4). To the Ga stock solution additional propan-2-ol and deionized water was added to obtain 20 vol% water content. This Ga dispersion was stirred at 1000 rpm at room temperature in a 250 mL glass beaker and the required volume of hexachloroplatinic acid solution in water (4.4 mg Pt mL−1) was added at once to obtain a Ga to Pt atomic ratio of 50. To keep the Pt concentration constant, the total volume was kept at 150 mL by adjusting the amount of Pt stock solution and additional water or propan-2-ol added. After completion of the galvanic displacement reaction, the resulting dispersion was centrifuged at 8000 rpm for 10 min. Then the supernatant was carefully removed, and the resulting Ga droplets were re-dispersed in 150 mL propan-2-ol. This washing step was repeated twice to remove most of the water and to obtain an almost water-free Ga/propan-2-ol dispersion. The resulting Ga droplets were then ultrasonicated (sonication bath) for 30 min to produce a well-dispersed Ga/propan-2-ol dispersion. This material was then deposited on Al2O3, dried under vacuum at 313 K using a rotary evaporator, and finally calcined for 2 hours at 773 K under ambient conditions to get the in situ prepared SCALMS-C* material (see Fig. 4).
Particle size analysis was performed using dynamic light scattering (DLS) measurements. For this purpose, the Ga dispersions were further diluted in clean propan-2-ol (ratio ∼ 1:20) and the resulting solution was analyzed using a Zetasizer device (Malvern Panalytical). The polydispersity index PDIDLS based on DLS measurements was calculated by taking the square of the ratio between standard deviation (STD) and mean value according to eqn (2).
(2) |
Transmission electron microscopy (TEM) images were recorded on an analytical Phillips CM30 TEM instrument using beam energy of 200 kV, equipped with a 2 K CCD camera. Samples were drop-casted onto a copper TEM grid, coated with a carbon film, and dried in a covered Petri dish before imaging.
Scanning Electron Microscopy (SEM) analyses were carried out using a Phenom Desktop SEM (BSD detector, 15 kV voltage). The particles were deposited directly on a conductive sticky carbon pad and dried under ambient conditions before measurement.
From the particle size vs. intensity graph (see Fig. 5a) it is seen that ultrasonication at 20% amplitude generates Ga droplets with larger particle size compared to the 40%, 60%, and 80% amplitudes. While ultrasonication at 20% and 60% produced Ga droplets with unimodal distribution, experiments with the 40% and 80% amplitudes resulted in bimodal distribution in our experiments. In terms of intensity-based harmonic mean, i.e., Z-average, 60% amplitude produced the lowest Z-average value of 206 nm, while at 80% the Z-average value was more than double at around 525 nm (see Table 1). When increasing the amplitude from 20% to 60%, the polydispersity index (PDIDLS) based on DLS measurements reduced from a value of 0.4 to 0.2 but further increasing the amplitude to 80% increased PDIDLS to ∼0.3. In all cases we produced Ga droplets population with a moderate polydispersity (PDIDLS = 0.1 to 0.4).
Amp./% | Z-avg./nm | PDIDLS/— | ||||||
---|---|---|---|---|---|---|---|---|
30 min | 60 min | 90 min | 120 min | 30 min | 60 min | 90 min | 120 min | |
Amp. = amplitude of sonication; Z-avg. = Z-average (intensity-based harmonic mean from DLS measurement); PDIDLS = polydispersity index based on DLS measurement. | ||||||||
20 | — | — | — | 525 | — | — | — | 0.40 |
40 | — | — | — | 277 | — | — | — | 0.24 |
60 | 264 | 248 | 213 | 206 | 0.31 | 0.27 | 0.22 | 0.20 |
80 | — | — | — | 249 | — | — | — | 0.29 |
The PDIDLS of the Ga droplets obtained in this work is comparable to the results reported by Yamaguchi et al.17 These authors, however, applied thiols as stabilizers. We also monitored the progression of Z-average and PDIDLS as a function of time at 60% amplitude (see Table 1).
Increasing the ultrasonication duration showed a positive effect in terms of reducing the Z-average as well as the PDIDLS. Increasing the ultrasonication duration from 30 to 90 min resulted in a 20% reduction in Z-average (from 264 nm to 213 nm) and in a 30% reduction in PDIDLS (from 0.31 to 0.22). Further increasing the duration to 120 min showed, however, only minor improvement in terms of both Z-average (from 213 nm to 206 nm) and PDIDLS (0.22 to 0.20). Lower Z-average and PDIDLS for 60% amplitude also became evident in the stability of the Ga-dispersion (see Fig. 5b and c and S1 in ESI†). The Ga-dispersion obtained with 60% amplitude was stable for 7 days while the one obtained with 20% amplitude settled in less than 24 hours. Therefore, we chose sonication at 60% amplitude for 120 min as our standard synthesis procedure for the following experiments.
The driving force for the formation of Ga–Pt nanostructures by the GDR can be described using the Nernst equation (see eqn (S1) in ESI† for details).32 From the standard reduction potential of Ga and Pt, it is clear that the reaction is spontaneous due to the large thermodynamic driving force (i.e. E0 = +1.267 V). Since Ga0 has the lowest oxidation potential compared to Pt4+, Ga0 gets oxidized and releases Ga3+ ions and electrons. The released electrons take part in the reduction of Pt4+ ions to Pt0 which leads to the formation of the Ga–Pt alloy on the surface of the liquid Ga droplet.28,29 When the GDR in propan-2-ol and aqueous environments were compared, significant differences were found in terms of Ga–Pt reaction kinetics as well as Ga–Pt nanocomposites morphology. It should be noted that the standard reduction potential of metal ions is defined in aqueous media and hence different reduction potential values in alcoholic solvents can be expected.49 Even though the determination of standard reduction potential is often complicated in alcoholic solvents, it is known that the standard potential of a given metal ion is directly related to its solvation energy. The standard reduction potential is more negative in a solvent in which the metal ion solvation is stronger.50 It can be assumed that this shift in standard reduction potential of Ga3+/Ga0 and Pt4+/Pt0 considerably reduces the thermodynamic driving force (i.e. E0 < +1.267 V) of the GDR in this solvent. This is the reason for the slower GDR in case of the reaction in propan-2-ol as seen in Fig. 6.
The difference in morphology between Ga–Pt nanocomposites formed in water-free propan-2-ol and in the two different water-containing dispersions is understood from the fact that the reduction or oxidation of metal ions can proceed via different routes depending on the applied solvent. The reduction of Cu2+ to Cu0, for example, occurs in one step in aqueous media, but in two steps in an aprotic solvent such as acetonitrile (via Cu2+ → Cu+ → Cu0).50 Such differences in reaction mechanism can lead to different morphologies during the GDR.49 Apparently, in the case of Ga–Pt GDR in propan-2-ol, the strong interaction of the Pt atoms dominates the GDR process leading to Pt island formation according to a classical Volmer–Weber growth model.49 In contrast, the two aqueous systems form Ga–Pt nanocomposites with uniform Pt dispersion.
Doping the Ga2O3/Al2O3 catalyst with Pt (Pt–Ga2O3/Al2O3) resulted in a material with the highest conversion level of all reference systems (approx. 28% after 3 h, see Fig. 8a). At the same time this catalyst exhibited enhanced cracking (48%) combined with significant aromatization (19%) and isomerization (17%) as shown in Fig. 8b). We also tested a commercially available, state-of-the-art, Pt/Al2O3 catalyst. Because of the high Pt loading (1.0 wt%) of the latter, the initial activity of this catalyst was around 31% but it deactivated to ∼16% over 12 h TOS, which is the highest rate of deactivation among all materials under investigation. The commercial catalyst gave rise to a n-heptene selectivity of 42%. Among all catalyst materials tested in this study, it exhibited the highest selectivity for cyclic product formation, while aromatic species were formed with only 9% selectivity.
In the next step, we studied the three different SCALMS catalysts under identical reaction conditions (Fig. 8c). For these experiments, we kept the Ga:Pt atomic ratio close to 50 since Ga50Pt alloys are liquid under the applied reaction conditions according to the Ga–Pt phase diagram.51 In the ex situ Ga52Pt SCALMS-A preparation, we worked with anhydrous propan-2-ol under an inert atmosphere to minimize the oxidation of the liquid Ga droplet surface. This catalyst showed high initial conversion (ca. 21%) but exhibited the most pronounced deactivation profile among the three SCALMS catalysts over time-on-stream. In terms of selectivity (see Fig. 8d), the desired formation of C7 n-alkenes was dominant (∼34%), followed by cracking (∼21%), isomerization (20%), and aromatization (∼9%). Thus, Ga52Pt SCALMS-A proved to be a reasonable dehydrogenation catalyst but in addition displayed significant cracking, isomerization, and aromatization activity.
For eutectic mixtures of Ga and In in water–ethanol mixtures Creighton et al.19 reported that water has a significant effect on the formation of the Ga2O3 passivation layer. The thickness of such layer increases with increasing water content.19 Therefore, we deliberately synthesized Ga54Pt SCALMS-B via galvanic displacement in pure water to produce a completely oxidized Ga surface. The resulting Ga54Pt SCALMS-B was the most active catalyst among the three systems, giving rise to stable conversion around 15% (see Fig. 8c). Note that the Pt loading in this material was 0.13 wt%, slightly less than the one in SCALMS-A with 0.15 wt%. The product distribution (see Fig. 8d) indicated that Ga54Pt SCALMS-B produced mainly cracked products (∼49%), aromatics (∼16%) and iso-alkanes/alkenes (∼16%). The selectivity towards the desired product n-heptene was low with only 8%. This selectivity pattern was in excellent accordance with the one for Pt–Ga2O3/Al2O3. This match suggests that the liquid Ga droplet surface here is indeed oxidized to a point where our standard H2 pretreatment procedure was not able to remove the Ga2O3 skin from the catalytic surface. Note that literature reports suggest that the Ga2O3 layer may also transform in presence of water to gallium oxide hydroxide (GaOOH) crystallites, which may also contribute to the observed reactivity.19
Our previous studies on propane dehydrogenation showed that the hydrogen formed in the initial phase of the process can reduce the Ga passivation layer, as the formation of water was observed.52 This process is facilitated by the presence of Pt that can indeed act as catalyst for the reduction of the Gallium oxide. However, under oxidative condition, as in pure water, the passivation layer may grow to such a thickness that even the performed pre-reduction step under pure H2 at 723 K could not completely remove the formed oxide, leaving the Ga droplets covered with a surface that is chemically analogue to a Pt–Ga2O3/Al2O3 catalyst.
The conclusion from our catalytic and analytic experiments to this point was that albeit water is needed for the GDR to form the desired Ga–Pt alloys, a pure water environment in the GDR is not suitable to produce a reducible SCALMS surface for the catalytic reaction. Hence, the right proportion of propan-2-ol and water was needed to speed up the GDR while minimizing the formation of thick Ga oxide layers on the supported Ga–Pt alloy. Consequently, we carried out the GDR in a propan-2-ol solution containing 20 vol% of water. For this reaction medium, our analytical experiments indicated fast GDR kinetics (see Fig. 6) and the formation of Ga–Pt nanocomposites with uniform Pt dispersion (see Fig. 7h and i). The resulting catalyst material (Ga53Pt SCALMS-C) showed a stable conversion of around 9% over the 14 h runtime. While this was the lowest activity level of all three catalysts, the n-heptene selectivity was highest with ∼63% (see Fig. 8d). At the same time, the cracking selectivity was low (∼9%), and other reaction such as cyclization (6%), aromatization (6%), and isomerization (9%) remained low. This selectivity pattern indicates the presence of active Pt sites in Ga53Pt SCALMS-C, where mainly the dehydrogenation of n-heptane to n-heptene proceeds. Competing acid–base activity originating from remaining Ga2O3 is largely suppressed in this Ga53Pt SCALMS-C due to the effective reduction of the thin Ga2O3 layer in the catalyst pretreatment process.
From the conversion and selectivity data, the cumulative productivity of each catalyst for the desired production of n-heptenes (in gn-heptenes gPt−1) can be calculated. Fig. 9 shows these values for the first 12 hours time-on-stream for all three SCALMS catalysts under investigation. The moderate n-heptene selectivity of Ga52Pt SCALMS-A resulted in a cumulative productivity of 630 gn-heptenes gPt−1, while the poor n-heptene selectivity of the very active Ga54Pt SCALMS-B yielded only 190 gn-heptenes gPt−1. The high n-heptene selectivity combined with high catalyst stability and reasonable activity of Ga53Pt SCALMS-C resulted clearly in the highest cumulative n-heptene productivity of 1230 gn-heptenes gPt−1 after 12 h time-on-stream.
In our improved SCALMS catalyst preparation – as shown in this study for Ga–Pt SCALMS-C – the Ga droplet oxidation is reduced to a minimum by a fast GDR. The resulting thin Ga2O3 passivation layer is mostly reduced during H2 pre-treatment and creates a clean interface, where Pt atoms are present in the liquid Ga matrix. This difference explains the high selectivity for C7 dehydrogenation and the formation of n-heptenes despite the relevant and stable conversion. In-line with our previous studies on SCALMS, we attribute the high stability of Ga–Pt SCAMS-C to the dynamic liquid–gas reaction interface and the single atom nature of the active Pt sites in this SCALMS material.9
We also compared the performance of Ga–Pt SCALMS prepared via ex situ and in situ GDR (see Fig. 3 and 4). For this SCALMS with similar Ga:Pt ratio (∼50) was prepared via in situ GDR, i.e., SCALMS-C* (see Table S4 in ESI† for composition). In catalytic testing under identical reaction conditions, we observed that in situ SCALMS-C* showed ca. 53% of the activity of ex situ SCALMS-C (see Fig. 10a).
The SEM analysis of the two materials did not show major difference (Fig. 11a and b), while EDX analysis showed a good correlation between Ga and Pt, confirming the bimetallic nature of the catalytic active phase (Fig. 11c and d and S8†) well in line with our previous investigation on Ga–Pt SCALMS.8
Fig. 11 SEM images of (a) SCALMS-C and (b) SCALMS-C* and EDX mapping of SCALMS-C* showing (c) gallium and (d) platinum. The scale bar represents 10 μm. |
However, the lower activity of this in situ prepared SCALMS can be attributed to a lower reactive interface due to a three-fold higher average Ga–Pt droplet size in the suspension used to prepare SCALMS-C* (see Fig. S3 in ESI†). We interpret the differences in Ga–Pt droplet size in the following way: the addition of hexachloroplatinic acid to the Ga dispersion in the in situ preparation route leads to the dissolution of the native oxide skin of the Ga droplets and this results in the coalescence of smaller droplets into bigger ones, similar to the report by Yamaguchi et al.17 On the contrary, the Ga droplets in the ex situ SCALMS synthesis route are already support stabilized which reduces the chance of droplet coalescence in the GDR step.
SCALMS-C* also showed a reduced selectivity for n-heptenes (52% vs. 63% for SCALMS-C). This latter aspect could be still due to the history of the sample: to deposit the bimetallic Ga–Pt droplets on the support, an extra sonication step in an ultrasonic bath was rendered necessary. In fact, the material after centrifugation was not readily dispersible due to strong droplet aggregation (see Fig. 4). This extra sonication step might trigger over-oxidation and/or dealloying, with detrimental effect on the performance of the final catalyst. Nevertheless, SCALMS-C* catalyst was significantly more selective towards n-heptenes than SCALMS-A and SCALMS-B (52% vs. 34% and 8%, respectively), confirming that the oxidation and nature of metallic phase plays a key role in n-heptane dehydrogenation reaction.
Finally, we investigated the effect of the Ga–Pt ratio in SCALMS-C materials from 27 to 99. Both Ga and Pt absolute masses in the reactor could not be kept constant but deviated by ±23% (Ga from 43 to 68 mg, Pt from 2.3 to 3.8 mg). Noteworthy, all SCALMS catalysts showed a similar conversion level between 9 and 10%, only the highly diluted Ga99Pt system was less active with only 6% at steady state conditions (see Fig. 12a). Interestingly, the selectivity of these five catalysts exhibited a maximum heptene formation for Ga53Pt, while at higher and lower ratios more cracking and cyclization occurred (see Fig. 12b). The combination of conversion and selectivity allowed the calculation of the n-heptene yield. As shown in Fig. 12c, the yield reached a maximum for Ga53Pt. The productivity, taking the different Pt loadings inside the reactor into account, also reached a maximum for Ga53Pt, after which it remained constant.
Fig. 12 a) Conversion over time in n-heptane dehydrogenation as function of the Ga–Pt ratio (all samples prepared according to the SCALMS-C protocol). b) Respective selectivity (at TOS = 12 h) in n-heptane dehydrogenation. c) Productivity and yield of heptenes obtained. d) Section of the Ga–Pt phase diagram according to Okamoto with liquidus line shown in red.51 Reaction conditions: 703 K, atmospheric pressure, 2.5 mL catalyst, H2/n-heptane = 8/1, 0.062 g min−1n-heptane, 118.87 mLN min−1 H2, 14.86 mLN min−1 He, 3320 mLgas gcat-bed−1 h−1 GHSV, ∼1.1 s residence time (τ). |
We interpret these findings with the help of the Ga–Pt phase diagram (see Fig. 12d).51 Ga–Pt systems with a Pt content of >4 at% are characterized by the presence of solid intermetallic Ga–Pt phases under the applied reaction conditions. Conversely, Ga–Pt systems with a Pt content of <2 at% are expected from the phase diagram to be fully liquid and form supported Ga–Pt liquid alloys under the reaction conditions. Ga–Pt systems with Pt contents between 2 and 4 at% contain solid intermetallics together with significant amounts of Pt in Ga liquid solution. We suggest, therefore, that the observed productivity enhancement up to a Ga–Pt ratio of 50 can be attributed to the fact that only above this level of Pt dissolution the presence of single Pt atom sites at the dynamic liquid–gas interface of the intermetallic phase is maximized.
By ultrasonication of Ga nuggets (0.5 g) in propan-2-ol (100 mL) at 60% amplitude for 120 min under ambient conditions, we were able to produce very stable Ga/propan-2-ol dispersions with an average Ga droplet size of 206 nm and PDIDLS of 0.20 without any stabilizers. The Ga–Pt galvanic displacement reaction (GDR) was spontaneous in water-containing systems (pure aqueous system or 20 vol% water in propan-2-ol) while the reaction in dry propan-2-ol solution was sluggish. It is assumed that the shift in standard reduction potential of Ga3+/Ga0 and Pt4+/Pt0 considerably reduces the thermodynamic driving force thus making the GDR in propan-2-ol less effective. TEM analyses of Ga–Pt nanocomposites synthesized in water-containing systems showed well-dispersed Pt in Ga matrix. GDR in propan-2-ol, in contrast, resulted in the formation of Pt aggregates on Ga droplet surface leading to island formation following a Volmer–Weber growth model.
During catalytic testing in n-heptane dehydrogenation, ex situ synthesized Ga–Pt SCALMS in pure propan-2-ol (i.e., Ga52Pt SCALMS-A) shows pronounced dehydrogenation and cracking activity. According to our TEM analyses, Ga52Pt SCALMS-A consists of large Pt crystallites formed on Ga droplets. The ex situ synthesized Ga–Pt SCALMS in pure water (i.e., Ga54Pt SCALMS-B) is a very effective cracking catalyst, an activity that is attributed to the presence of a bulk, non-reducible Ga2O3 on the catalyst material. Interestingly, ex situ synthesized Ga–Pt SCALMS in water/propan-2-ol (i.e., Ga53Pt SCALMS-C), shows impressive dehydrogenation activity with n-heptenes selectivity of 63% and suppression of side reactions. This attractive performance is attributed to the liquid alloy interface in Ga53Pt SCALMS-C with minimal Ga2O3 content and clean Pt single-atom active sites. The in situ synthesized Ga–Pt SCALMS showed less activity compared to their ex situ counterparts due to higher average droplet size and thus a lower reaction interface. The slightly lower selectivity of in situ SCALMS is presumed due to the post-GDR sonication step which could result in over-oxidation and/or dealloying.
We are convinced that our findings will pave the way towards a rational development and effective production of SCALMS materials using ultrasonication. Given its simplicity and excellent atom efficiency, we anticipate that this preparation method will develop into the preferred choice to produce SCALMS materials for larger-scale, technical applications in the future.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3cy00356f |
This journal is © The Royal Society of Chemistry 2023 |