Li-Ling
Chiu
a and
Sheng-Heng
Chung
*ab
aDepartment of Materials Science and Engineering, National Cheng Kung University, Tainan 701, Taiwan
bHierarchical Green-Energy Materials Research Center, National Cheng Kung University, Tainan 701, Taiwan. E-mail: SHChung@gs.ncku.edu.tw
First published on 23rd May 2022
Lithium–sulfur batteries with a high-capacity cathode and high cell energy density have been regarded as next-generation energy-storage systems because of their suitability for high-energy-density devices with a low cost. However, the intermediate lithium polysulfides easily dissolve in liquid electrolytes and irreversibly diffuse from the cathode. In this study, we develop a high-loading polysulfide cathode featuring a polymethyl methacrylate (PMMA)-based gel-polymer electrolyte (GPE). The PMMA-based GPE inhibits the diffusion of liquid polysulfides by the strong chemical bonding between the carbonyl groups of the GPE and lithium sulfides, while offering high lithium-ion transfer for the high-loading cathode to attain outstanding electrochemical performance. Moreover, to investigate and increase the lithium-ion conductivity of the GPE, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) is mixed with PMMA at five concentrations. Material and electrochemical analyses reveal that under a high sulfur loading of 4 mg cm−2, the cell with the PMMA-based GPE containing 90 wt% PMMA and 10 wt% LiTFSI exhibits the lowest impedance and highest electrochemical utilization and stability. In addition, the PMMA-based GPE allows the cell to attain higher sulfur loadings (8 and 10 mg cm−2), while exhibiting a high areal capacity of 7.1 mA h cm−2 and a high energy density of 15 mW h cm−2. Therefore, the PMMA-based GPE enhances the electrochemical stability and improves the efficiency and safety of the high-loading polysulfide cathode, which are the key factors for high-energy-density lithium–sulfur cells.
Besides the insulating nature of the solid active material, an additional problem is that lithium polysulfide as the intermediate product is a liquid active material with high solubility in liquid electrolytes, which can rapidly degrade the reversible capacity and stability of the cell. Thus, polymers have been widely used in battery research as energy materials, separators, and interlayers.14,15 Solid-polymer electrolytes (SPEs) and gel-polymer electrolytes (GPEs) are promising solutions to inhibit the dispersal of liquid-state polysulfides and improve the stability of lithium–sulfur batteries.16,17 Although SPEs can inhibit the diffusion of liquid polysulfides, the low conductivities and high room-temperature resistance of polymers still limit the development of SPEs.18 Polymer matrices have high affinity toward liquid electrolytes, which can reduce interfacial resistance;19 therefore, many researchers have reported that GPEs such as polyethylene oxide,20 polyacrylonitrile,21 polymethyl methacrylate (PMMA),22 and poly(vinylidene fluoride-co-hexafluoropropylene)23 can inhibit the diffusion of lithium polysulfide, while improving the electrochemical stability and maintaining high electrochemical utilization of lithium–sulfur cells.19,24 In addition to the material design, in recent studies, GPEs have been investigated by wide fabrication techniques, including casting, electrospinning, functional group grafting, or additive introduction to inhibit lithium polysulfide diffusion and improve the battery electrochemical performance. Ester-based polymers that can strongly interact with lithium polysulfides and inhibit polysulfide diffusion have recently been reported.22 Among the ester-based polymer candidates, PMMA (R–COO–R′) endows lithium-ion batteries with high ionic conductivity because of its good affinity for organic electrolytes.25
Moreover, to tackle the chemistry and engineering issues of batteries, lithium–sulfur battery cathodes require a high active-material loading and content attaining 4–10 mg cm−2 and 60–80 wt%, respectively. With such optimal cell-design parameters, the sulfur cathode would be able to achieve a desirable electrochemical performance with high areal capacity and energy density.26–28 Thus, GPEs that have high ionic conductivity and inhibit the diffusion of liquid polysulfides would be useful for high-loading sulfur cathodes to attain high utilization of the active material and retain liquid polysulfides in the cathode region of the cell.
Herein, we addressed the above-mentioned issues in GPEs and in lithium–sulfur technology by developing a PMMA-based GPE to allow a high-loading polysulfide cathode with enhanced electrochemical utilization and reversibility. We first fabricated the PMMA-based GPE with PMMA and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) integrated to a polymeric separator. PMMA, which features a carbonyl group (–CO), has high binding energies to liquid polysulfides and Li2S.29 LiTFSI can improve the ionic conductivity of GPEs.20 The polymeric separator offers the skeleton of the GPE membrane. We investigated five different concentrations of LiTFSI (i.e., 0, 5, 10, 15, and 20 wt%) to compare the material characteristics and electrochemical performances of different PMMA-based GPEs, which further demonstrated the optimal GPE design. Our analytical results confirm that the PMMA-based GPE with 90 wt% PMMA and 10 wt% LiTFSI provided the cell with the highest initial discharge capacity (1038 mA h g−1) and best electrochemical performance at a high sulfur loading of 4 mg cm−2 and C-rate of C/10. Subsequently, to prove that the PMMA-based GPE can inhibit liquid polysulfide diffusion, we further increased the sulfur loading to 8 and 10 mg cm−2. The PMMA-based GPE demonstrated a smooth electrochemical reaction and high capacity retention. With the high electrochemical utilization and reversibility, the PMMA-based GPE allowed the high-loading polysulfide cathode to achieve a high areal capacity and a high energy density, outperforming the current standard for lithium-ion battery cathodes.
The assembled cells were tested at room temperature. The voltage window of cycling performance, rate performance, and charge/discharge curves were collected using a programmable battery cycler (CT-4008-5 V–10 mA, Neware) at 1.8–2.8 V and a C-rate of C/10. Furthermore, cyclic voltammetry (CV) analysis was conducted using a potentiostat (VMP-300, Biologic) at the same working voltage, but different scan rates: 0.010, 0.015, 0.020, and 0.025 mV s−1. Electrochemical impedance spectroscopy (EIS) data were recorded from 1 MHz to 10 mHz using an impedance analyzer (SP150, Biologic), at an AC voltage amplitude of 5 mV and open-circuit voltage. Additionally, the room temperature ionic conductivity value was tested at a frequency of 1 MHz to 100 Hz. Through the equation (σ = d/A × Rb) about ionic conductivity, d, A and Rb meant the thickness, area, and bulk resistance of the PMMA-based GPE, respectively.
Moreover, the Raman spectroscopy data of the chemical interaction between PMMA and LiTFSI are presented in Fig. 1 and Table 1. The carbonyl group on PMMA strongly interacts with lithium ions.22,25,29 The absence of the peaks of carbonyl and TFSI− anion groups in the GPE sample with 10 wt% LiTFSI indicates that no redundant carbonyl groups or TFSI− anion groups remained inside the GPE. In contrast, the spectrum of the PMMA-based GPE without LiTFSI featured a peak at 1729 cm−1 due to the absence of lithium salts, whereas the spectra of the GPEs with 15 and 20 wt% LiTFSI featured a peak at 741 cm−1, indicating an overdosage of lithium salts.33 Therefore, the LiTFSI concentration in PMMA-based GPEs is an important factor in forming a lithium-ion transfer network, and 10 wt% was the optimum concentration in this regard. The morphologies of the prepared PMMA-based GPE samples are shown in Fig. S3.† The GPE samples with the five LiTFSI concentrations had a uniform and smooth surface, consistent with the findings of a previous study.22 This confirms the casting method as a suitable GPE fabrication method. Moreover, the contents of PMMA and LiTFSI would be the main factor for improving the electrochemical performance of the lithium–sulfur cell with a high-loading polysulfide cathode.
Raman band (cm−1) | Assignments |
---|---|
602 | ν(C–COO), νs (C–C–O) |
741 | TFSI− |
853 | ν(CH2) |
999 | O–CH3 rocking |
1081 | ν(C–C) |
1264 | ν(C–O), ν(C–COO) |
1460 | δ a (C–H) of α-CH3, δa (C–H) of O–CH3 |
1729 | ν(CO) of (C–COO) |
2848 | Combination band involving O–CH3 |
2957 | ν s (C–H) of O–CH3 with νs (C–H) of α-CH3 and νa (CH2) |
3001 | ν a (C–H) of O–CH3, νa (C–H) of α-CH3 |
To elucidate the chemical bonding between PMMA and the LiTFSI salt, the 1H and 7Li solid-state nuclear magnetic resonance (NMR) spectra are shown in Fig. S4.† Solid-state NMR has less sensitivity than liquid-state NMR; therefore, the H atoms of PMMA overlapped. The 1H solid-state NMR spectra (Fig. S4a†) featured broad peaks and inconspicuous shifts. Moreover, a comparison of the 7Li solid-state NMR spectra of the LiTFSI salt and PMMA-based GPE indicated lithium ions connected with the carbonyl group of PMMA so that the peaks shifted leftward, as reported in previous research.34 The interaction between the lithium ions and carbonyl groups can be expected to facilitate lithium-ion transmission in the PMMA-based GPE.
The experimental and analytical electrochemical impedance spectroscopy (EIS) plots of the lithium–sulfur cells with PMMA-based GPEs featuring different PMMA-to-LiTFSI ratios before and after cycling are illustrated in Fig. 2b and c. Re, Ri, and Rct represent the bulk resistance of electrodes and electrolyte, interface resistance, and charge-transfer resistance, respectively. Warburg impedance (Zw) is attributable to lithium-ion diffusion. Before cycling, the Rct and Ri values of the lithium–sulfur cells applying the PMMA-based GPEs with PMMA:LiTFSI ratios of 100:0, 95:5, 90:10, 85:15, and 80:20 wt% were 294.9 and 46.9 Ω, 140.3 and 85.9 Ω, 76.8 and 14.3 Ω, 169.7 and 32.3 Ω, and 218.7 and 59.2 Ω, respectively. Therefore, the addition of the appropriate quantities of LiTFSI salt decreased the charge-transfer resistance and interface resistance, whereas the addition of excessive LiTFSI increased the charge-transfer and interface resistances and limited the electrochemical abilities of the lithium–sulfur cells. After cycling, the high frequency charge-transfer impedance of the cells was reduced, because active materials were kinetically rearranged during the electrochemical reaction. Specifically, Rct at a high frequency decreased to 31.1, 46.8, 22.4, 28.7, and 25.6 Ω with PMMA:LiTFSI ratios of 100:0, 95:5, 90:10, 85:15, and 80:20 wt%, respectively. Moreover, the corresponding Ri at a low frequency was 6.6, 1.7, 7.7, 14.0, and 11.7 Ω, respectively.
As a result, under a high sulfur loading of 4 mg cm−2, the PMMA-based GPE with an LiTFSI concentration of 10 wt% endowed lithium–sulfur cells with excellent electrochemical cyclability and stability, compared with the cells with other LiTFSI concentrations. Moreover, the PMMA-based GPE with 10 wt% LiTFSI salt exhibited the lowest electrochemical resistance in cells. All these positive features therefore affirm that the optimal LiTFSI concentration for the PMMA-based GPE in advancing lithium–sulfur cells was 10 wt%.
Fig. 3a displays the electrochemical cyclabilities of high-sulfur-loading lithium–sulfur cells. The initial and reversible discharge capacities after 100 cycles of the cells with increasing high sulfur loadings of 4, 8, and 10 mg cm−2 were 1038 and 641 mA h g−1, 797 and 502 mA h g−1, and 708 and 515 mA h g−1, respectively. Even the cell with an ultrahigh sulfur loading of 10 mg cm−2 can have a high capacity retention of 73% after 100 cycles. However, due to the electrochemical reaction of lithium–sulfur batteries, the conversion reaction of active materials between sulfur, polysulfides, and sulfides would continuously consume the electrolyte and the added LiNO3 co-salt, which causes the initial decrease of the discharge/charge efficiency.26 In our study, the cell with the PMMA-based GPE contained a high amount of sulfur and had the GPE system, which might lead to the initial decrease in the discharge/charge efficiency, while the cell then maintained a stable and high efficiency during the subsequent long cycle life. Moreover, although the utilization of sulfur slightly decreased from 62%, 48%, and to 42% with the increasing high sulfur loadings from 4, 8, and to 10 mg cm−2 and the corresponding high sulfur contents from 52, 68, and to 72 wt%, the high-sulfur-loading polysulfide cathode eventually exhibited a high areal capacity and energy density of 7.1 mA h cm−2 and 15 mW h cm−2, respectively. These performance values are higher than those of a commercial lithium-ion battery cathode (e.g., 2–4 mA h cm−2 and 10–15 mW h cm−2).1–5
Fig. 3 Electrochemical analysis results of high-sulfur-loading cells: (a) cyclability; (b) rate performance at a sulfur loading of 10 mg cm−2; and EIS images (c) before and (d) after cycling. |
Fig. 3b presents the high rate performance of the PMMA-based GPE modified lithium–sulfur cells with a high sulfur loading of 10 mg cm−2. The high-loading polysulfide cathodes with the PMMA-based GPE exhibited excellent reversible discharge capacities of 717, 605, 507, 428, and 318 mA h g−1 at C/20, C/10, C/5, C/3, and C/2 (1C = 1675 mA g−1) after 10 cycles, respectively, with high and stable discharge/charge efficiency. The cycled cell was subsequently returned to C/10 and subjected to 50 additional cycles. The cell still exhibited a high discharge capacity, which indicates that the PMMA-based GPE could confine liquid polysulfides in the cathode and inhibit their diffusion even if a high amount of polysulfide existed and was generated in the high-loading polysulfide cathode. In order to further support this result, we observed the cycled PMMA-based GPE composite from its anode side, which showed no trace of polysulfide diffusion and no deposition of sulfur or sulfide (Fig. S6†). Therefore, lithium–sulfur cells with a PMMA-based GPE can preserve the active material and undergo high-reversibility electrochemical reactions.
As a reference, a summary of the discharge/charge curves of the rate performance analysis is displayed in Fig. S7.† Although the cells contained a high amount of liquid polysulfide catholyte as the active material, the lithium–sulfur batteries still exhibited a smooth electrochemical reaction. To support these outstanding cell performances, we subsequently conducted electrochemical EIS and CV analysis to explore the electrochemical stability and reversibility as well as the reaction kinetics of the high-loading polysulfide cathode with the PMMA-based GPE. Moreover, we further studied the room temperature ionic conductivity values of the PMMA-based GPEs before and after soaking the electrolyte (Fig. S8†). The ionic conductivity of the PMMA-based GPE precursor was 1.66 × 10−4 S cm−1 before soaking the liquid electrolyte. After the GPE precursor absorbs the electrolyte, the ionic conductivity of the resulting PMMA-based GPE increases to 2.44 × 10−2 S cm−1.
Fig. 3c and d present the experimental and analytical EIS data of high-loading polysulfide cathodes with the PMMA-based GPE. With increasing sulfur loadings, Rct increased, attributable to the insulating properties of sulfur and the high-amount of polysulfide in the cathode. Before cycling, the cells with sulfur loadings of 4, 8, and 10 mg cm−2 exhibited Rct values of 76.8, 85.1, and 123.7 Ω, respectively. After 100 cycles, the Rct values became lower: 22.4, 26.4, and 33.5 Ω, respectively. Furthermore, the Ri values of the batteries with sulfur loadings of 4, 8, and 10 mg cm−2 at a low frequency changed from 14.3, 16.5, and 13.7 Ω to 7.7, 23.8, and 4.8 Ω after 100 cycles. The fresh cells shown in Fig. 3c have a high resistance because of the high amount of the insulating active material on the current collector. Thus, the fresh cells showed a high impedance. After 100 cycles, as shown in Fig. 3d, the cycled active material rearranged and occupied a more electrochemically favorable position. This suggests a closer contact and better coverage between the physically stable active material on the current collector and the GPE, which results in the decrease of the impedance.10 This further indicates that the PMMA-based GPE inhibited liquid-polysulfide diffusion and facilitated electrochemical kinetics. On the other hand, the high sulfur loading and content in the cathode also impact the resulting EIS data. The cell with the highest sulfur loading of 10 mg cm−2 hosted the highest amount of insulating sulfur (10 mg cm−2 and 72 wt%), which showed the high charge transfer resistance at high frequency. The interface resistance at low frequency would be hard to detect and covered by the high charge transfer resistance. Moreover, the high-loading sulfur cathode inevitably encountered a relatively low sulfur utilization. Thus, the resulting deposition of the converted solid active material might not be as much as that of the high-loading sulfur cathode with a sulfur loading and content of 4 mg cm−2 and 52 wt% and 8 mg cm−2 and 68 wt%. According to these two reasons, the cell with the highest sulfur loading was found with a low interface resistance and high charge transfer resistance after cell cycling.
To further clarify the enhanced electrochemical performances of the PMMA-based GPE in lithium–sulfur cells, cyclic voltammetry (CV) tests were performed at four rates (0.010, 0.015, 0.020, and 0.025 mV s−1; Fig. 4a–c). The CV curves featured two cathodic peaks (i.e., Li2S8/S8 → Li2S4–8 and Li2S4–8 → Li2S2/Li2S) and one broad anodic peak (i.e., Li2S2/Li2S → Li2S8/S8). The cells were scanned two times with the increase of the scan rate, which displays each CV curve featuring two perfect reversible cycles (Fig. S9–S11†). With a high amount of sulfur of 4 to 10 mg cm−2 and also the increase of the corresponding sulfur content in the cathode from 52 to 72 wt%, the polarization of the cell increased as found in the CV data, which cause the differences in the oxidation peaks.21 However, the redox reaction of our high-loading polysulfide cathodes with the PMMA-based GPE still displays high electrochemical stability and reversibility at various scan rates.
Fig. 4 Cyclic voltammograms of high-sulfur-loading cells: (a) 4 mg cm−2; (b) 8 mg cm−2; (c) 10 mg cm−2. |
Additionally, the lithium-ion diffusion coefficient could be calculated using the Randles–Ševčík equation (Fig. S9e, S10e, and S11e†). As the high sulfur loading increased from 4 to 10 mg cm−2, the lithium-ion diffusion coefficients slightly decreased from 5.27 × 10−9–3.1 × 10−8 cm2 s−1 to 2.09 × 10−9–1.27 × 10−8 cm2 s−1, while remaining high. The retention of relatively high lithium-ion diffusion coefficients in the high-sulfur-loading cathodes indicated that the PMMA-based GPE resulted in high ionic conductivities and high lithium-ion transfer between the cathode and anode. Therefore, the PMMA-based GPE enhanced the lithium-ion transfer and inhibited polysulfide diffusion, which can limit the loss of the active material, enhance the electrochemical performance of cells, and enhance sulfur utilization.
Furthermore, we compared the studied lithium–sulfur batteries containing our PMMA-based GPE with literature-reported batteries containing other GPEs to show the development of the GPE in lithium–sulfur cells (Fig. 5). The comparison aims to summarize the research trends in terms of cell-design parameters (i.e., sulfur loading and sulfur content) and the corresponding cell-electrochemical performances (i.e., the areal capacity and energy density), which together lighten the direction toward advanced lithium–sulfur batteries with a high-energy-density sulfur cathode and a high-performance safe GPE.
Specifically, as shown in Fig. 5a, the cells with the PMMA-based GPE enable the high-loading polysulfide cathodes to simultaneously attain high sulfur loading (10 mg cm−2) and sulfur content (72 wt%), showing the improvement in the sulfur cathode in the GPE system. Moreover, as shown in Fig. 5b, with such a high-loading polysulfide cathode, the PMMA-based GPE allows the enhanced electrochemical performance featuring a high areal capacity of 7.1 mA h cm−2 and excellent energy density of 15 mW h cm−2, which promotes the development trend as compared to the previous studies. As a result, the comparison analysis shows a summary of various lithium–sulfur GPEs. The analytical results also demonstrate that our PMMA-based GPE attains the achievements in both cell design (i.e., high sulfur loading and content) and cell performance (i.e., outstanding areal capacity and energy density).
Footnote |
† Electronic supplementary information (ESI) available: Material analyses with contact angles, FTIR, SEM, and NMR for PMMA-based GPEs; electrochemical analysis with discharge/charge curves, ionic conductivity, and CV analysis for the cells with PMMA-based GPEs; and supporting references. See https://doi.org/10.1039/d2ta01867e |
This journal is © The Royal Society of Chemistry 2022 |