Kenneth G.
Latham
*ab,
Marveh
Forghani
c,
Wesley M.
Dose
de,
Jessica A.
Allen
f and
Scott W.
Donne
a
aDiscipline of Chemistry, University of Newcastle, Callaghan, NSW 2308, Australia. E-mail: kenneth.latham@umu.se
bUmeå University, Department of Chemistry, SE-90 187, Umeå, Sweden
cInstitute of Future Transport and Cities, Coventry University, Priory Street, Coventry CV1 5FB, UK
dDepartment of Chemistry, University of Cambridge, Lensfield Road, Cambridge, CB2 1EW, Cambridge, UK
eDepartment of Engineering, University of Cambridge, 17 Charles Babbage Road, CB3 0FS, Cambridge, UK
fSchool of Engineering, University of Newcastle, Callaghan, NSW 2308, Australia
First published on 7th December 2020
Ammonium has been successfully utilized to nitrogen dope carbon structures via hydrothermal carbonization, although the influence of different attached counter ions (anions) on the resultant carbon physicochemical properties and electrochemical performance has not been examined before. Four different counter ions (SO42−, PO43−, Cl−, and Fe(SO4)2) attached to ammonium were seen to influence the hydrothermal reaction, nitrogen incorporation levels, physicochemical properties, activation ability and supercapacitor performance. For instance, nitrogen K-edge NEXAFS found differences in the levels of pyridinic and pyrrolic groups with PO43− incorporating predominately pyridinic nitrogen groups. PO43− also achieved the highest surface area (2132.6 m2 g−1), however this material was unstable as a supercapacitor, losing almost 50% of its performance over 500 cycles. SO42− resulted in the highest level of nitrogen incorporation (5.53 at%) and hydrothermal yield (45.5%), while Fe(SO4)22− resulted in the lowest (2.92 at%). However, Fe(SO4)22− produced unique flower like structures not seen in any of the other anions. Cl− produced the highest performing material, achieving 190 F g−1 at 10 mV s−1 in 1 M KOH and had moderate nitrogen incorporation (3.42 at%). Overall, this study indicates that the anion has substantial influence on the physicochemical properties of the material, allowing an additional level of tailoring.
Among the heteroatom doped carbon materials, nitrogen is by far the most prominent dopant for its enhancement of electronic conductivity,7 improved surface wettability through hydrophilic groups and increased surface roughness,5 as well as ease of incorporation into carbon materials through a wide range of methods.3 Incorporating pyridinic, pyridonic, pyrrolic and oxidized –NOx, groups has been suggested to create sites where reversible faradaic redox reactions (pseudocapacitance) can occur, providing additional charge storage sites.3,9 Quaternary or graphitic nitrogen is also possible and suggested to promote the transport of electrons through the carbon lattice, reducing resistance.3
Nitrogen doped carbon materials have also shown promise in enlarging the cell voltage window, with Chi et al. showing excellent stability and capacitance retention of a nitrogen doped carbon surface after a 10000-cycle floating-like test between 3 and 4 V using an organic electrolyte (1 M TEABF4/PC).10 For comparison, the upper cut off voltage for CSC using organic electrolytes is generally between 2.5–2.7 V.11 As a result, nitrogen doped materials have consistently outperformed their non-doped counterparts when used in supercapacitors.
Several approaches exist for synthesizing nitrogen doped carbon materials, such as chemical vapor deposition,12,13 plasma5 and arc discharge,14 pyrolysis of nitrogen containing precursors15,16 and hydrothermal carbonization.17,18 However, it is important to ensure that the production method is sustainable and environmentally friendly. For this reason, hydrothermal carbonization, a low temperature wet carbonization method,19 is preferred and excels in producing highly nitrogen doped carbon materials with a range of nitrogen functionalities.17,18,20,21
Using hydrothermal carbonization, nitrogen doped carbon materials can be synthesized by directly carbonizing nitrogen containing precursor (e.g., tannin,22 microalgae,23,24 chitosan21,25) or reacting a carbonaceous precursor (e.g., glucose, biomass) in the presence of a nitrogen containing agent (e.g., ammonium salt,17,26 ammonia,18 urea,27 glycine28). The first approach is simpler, although this provides limited control over the degree of nitrogen incorporation, precursor materials or the types of nitrogen groups formed. The second approach provides a greater level of flexibility with the nitrogen level and type being independent of the main carbon source. For instance, Park et al. demonstrated that the type and amount of nitrogen functional groups could be easily adjusted through modifying ratio between the nitrogen and non-nitrogen containing precursors as well as the reaction temperature.29 Additionally, nitrogenation agents containing multiple elements (e.g., (NH4)2HPO326,30) can further enhance the material beyond the influence of nitrogen via synergistic co-doping effects. For instance, phosphorus has a higher n-type behavior and stronger electron expansion ability than nitrogen, which can generate additional charge storage areas and improve electrical conductivity.31 Phosphorus doped carbons have also been shown to have larger stable voltage windows.32 Chlorine functionalization was shown by Pinkert et al. to increase the specific capacitance by 27% over a non-doped carbon at a cycle rate of 10 mV s−1 in EMIBF4 from −3.4 V to 3.4 V.33 Thus, co-doping is a way to further enhance the carbon surface beyond nitrogen doping. It is for this reason that ammonium salts represent an interesting group of compounds for enhanced hydrothermal doping, which have already been shown to co-dope carbon materials via hydrothermal carbonization.34 However, former studies examining the hydrothermal carbonization of glucose, fructose and sucrose with (NH4)2SO4 and (NH4)2HPO4 indicated that the ammonium counter-ion (anion), has an influence on the hydrothermal reaction.30 This study found vast differences in yield and pH between the (NH4)2SO4, (NH4)2HPO4 and non-doped hydrothermally carbonized materials.30
In this study we have examined the influence of four ammonium salts, (NH4)2SO4, (NH4)2HPO4, NH4Cl and (NH4)2Fe(SO4)2·6H2O on the hydrothermal carbonization of sucrose and supercapacitor performance. Extensive surface studies were conducted via XPS and synchrotron based NEXAFS to understand the differences in surface functionalities on the hydrothermal materials and activated hydrothermal materials. These surface studies were correlated with in-depth electrochemical studies using step potential electrochemical spectroscopy (SPECS), which can identify the different charge storage mechanisms occurring on these materials.35,36
Surface area and porosity was examined by gas adsorption using a Micromeritics ASAP 2020 Surface Area and Porosity Analyzer. A representative 0.10 g sample of the carbon material was degassed under vacuum at 110 °C for 2 hours prior to analysis. An adsorption isotherm was then determined over the partial pressure range of 10−7–1 using N2 gas as the adsorbate at 77 K. The specific surface area was extracted from the gas adsorption data using the linearized BET isotherm in the partial pressure range 0.05 < P/P0 < 0.3.37
The recorded signal was normalized to the incident photon flux using the stable monitor method, in which the sample signal is compared consecutively to clean reference samples and the time variation in flux is measured via a gold mesh.40 The normalized spectra were scaled by setting the pre-edge signal (280 eV for carbon and 380 eV for nitrogen) to zero and the post edge (320 eV for carbon, 415 eV for nitrogen) to 1. The photon energy was calibrated by measuring the NEXAFS spectrum of HOPG simultaneously to the sample signal and normalizing to the excitation peak at 291.65 eV.
To understand the effects of synchrotron radiation beam damage on the hydrothermal carbons, a sequence of scans was initially measured on the same spot until significant changes were observed in the carbon and nitrogen K-edge spectra. The scan time was subsequently restricted to an appropriate interval below this (∼0.5 s per 0.1 eV step) in which beam damage during a single scan was negligible.
The counter electrode was prepared using a similar method except the activated hydrothermal carbon was replaced with carbon black conductive agent (Cabot, Vulcan XC72R) giving a weight ratio of 95:5 carbon black to PTFE. Additionally, 160 μL of the counter electrode ink was drop cast onto the stainless steel rod to ensure a greater mass of electrode material than the working electrode. The working electrodes weighed ∼4 mg cm−1, whereas the counter electrodes weighted ∼11.8 mg cm−1. This ensured that any limitations in the system were the result of the working electrode. Both electrodes were dried under air at 60 °C for 8 hours, the average mass of active material contained in the working electrodes was 3.3 ± 0.2 mg cm−1.
The specific capacitance (Cs, F g−1) was calculated from the CV curves according to the following equation:
The influence of the aforementioned factors can be observed in Table 1, where the yield of hydrochar and solution pH change with different counter-ions. The differences in initial pH are due to how each ammonium salt disassociates in solution, for instance, the ammonium ion disassociates in ammonium chloride via the following equilibrium:
Cl− + NH4+ + H2O ⇌ NH3 + H3O+ + Cl− |
2NH4+ + HPO4 ⇌ NH3 + NH4+ + H2PO4 |
NH4+ + H2PO4 ⇌ NH3 + H3PO4 |
Sample | Yield (%) | Yield – AWa (%) | pH initial | pH final | H+ produced (mM) | Average particle diameter (μm) |
---|---|---|---|---|---|---|
a Yield remaining after washing with acetone. b Particle size was not calculated as individual particles were not present. | ||||||
H-Con | 29.6 ± 1.0 | 22.1 ± 0.02 | 5.72 ± 0.02 | 2.35 ± 0.02 | 4.4 ± 0.2 | 4.57 ± 1.15 |
H-SO | 45.5 ± 0.5 | 44.7 ± 0.02 | 5.36 ± 0.02 | 0.92 ± 0.02 | 121.6 ± 5.6 | 4.12 ± 0.95 |
H-Cl | 28.8 ± 1.1 | 27.8 ± 0.01 | 5.15 ± 0.01 | 1.12 ± 0.01 | 75.4 ± 1.7 | 4.01 ± 1.77 |
H-Fe | 42.6 ± 0.7 | 41.2 ± 0.01 | 3.02 ± 0.01 | 1.08 ± 0.03 | 83.2 ± 5.8 | 3.46 ± 1.34 |
H-PO | 35.2 ± 0.2 | 34.7 ± 0.02 | 8.58 ± 0.02 | 2.44 ± 0.04 | 3.7 ± 0.3 | NAb |
The creation of H2PO4 and H3PO4 has a buffering effect within the solution, increasing the pH. The pH decreased for every sample during hydrothermal carbonization, indicating the formation of acidic species. For saccharides, this tends to be formic, lactic, acetic, propanoic and levulinic acid.30 The addition of (NH4)2SO4, NH4Cl and (NH4)2Fe(SO4)2 lowered the pH to around 1, however this is unlikely to be the result of increased organic acid production as the pKa of the above-mentioned organic acids are from 3.75 to 4.87, indicating that these compounds are likely to be in their protonated form. This is more likely to be due to the formation of H2SO4 and HCl in the liquid as NH4+ is consumed by the carbonization process, leaving free SO42− and Cl− ions.
The observed differences in hydrochar yield are most likely from the ammonium counter ion, and not the influence of NH4+ or the influence of pH. NH4+ concentration was the same for all of the hydrothermal solutions and the pH is similar in H-Cl and H-Fe, but the yield of H-Cl is 28.8% whereas H-Fe is 42.6%. The reason for the increase in yield for H-SO and H-Fe has been ascribed to the presence of SO42− in the solution, which has been shown to accelerate the carbonization process from the saccharide to intermediates.46 Additionally, Ming et al. found that the addition of Na+ and SO42− to the hydrothermal solution in the form of Na2SO4 created aromatic species in the solution that were not observed without salt addition.46 This suggested that Na2SO4 could play a catalytic role in accelerating the conversion of intermediates to carbon materials. However, they did not examine whether these aromatics were present with NaCl or NaNO3 added, thus it is unclear if the effect is from the anion (SO42−) or the cation (Na+). Considering that we have compared the anions in this study and seen that SO42− increases the yield of over Cl and PO43−, this indicates that SO42− is the reason for the increased yield. Additionally, Lu et al., found that the presence of NaCl increased the conversion to intermediates, but not the final yield of carbon material,47 further demonstrating that it is the presence of SO42− and not Na+ that promotes the formation of carbon.
Changing the counter-ion also resulted in morphological differences (Fig. 1). H-Con, H-Cl, H-Fe and H-SO all displayed spherical particles with an average diameter of 3.46 ± 1.34 μm for H-Fe to 4.57 ± 1.15 μm for H-Con, whereas H-PO consisted of a conjoined structure. Interestingly, the incorporation of (NH4)2FeSO4 in H-Fe also resulted in the formation of ‘flower-like’ structures appearing alongside the commonly observed spherical particles.
The surface area (Table 2) for the non-activated materials was <21 m2 g−1 for all samples, a typical result for hydrothermally derived carbon from saccharides as they contain almost no porosity.
Sample | BET surface area (m2 g−1) | Micropore surface area (m2 g−1) |
---|---|---|
H-Con | 21 | 2.5 |
H-SO | 3 | 0.5 |
H-Cl | 16 | 2.7 |
H-Fe | 3 | 0.6 |
H-PO | 10 | 3.6 |
A-Con | 1517 | 320 |
A-SO | 738 | 172 |
A-Cl | 1968 | 384.8 |
A-Fe | 667 | 160.5 |
A-PO | 2133 | 419.3 |
Activation with H3PO4 consists of two equally important stages, impregnation and carbonization. Increasing the impregnation or carbonization time increases the surface area of the materials, as impregnation time allows H3PO4 to penetrate further into the material and carbonization time allows for micro porosity development.48 The activation process (Fig. 1(g) and (h)) roughened the surface, chipping off sections of the spherical particles and forming small cracks. This can easily be observed by comparing the spherical particle of H-SO in Fig. 1(f) with the activated spherical particle of A-SO in Fig. 1(h). Specific surface area increased in the order of A-Fe (667 m2 g−1), A-SO (738 m2 g−1), A-Con (1517 m2 g−1), A-Cl (1968 m2 g−1) and A-PO (2133 m2 g−1). The differences in surface area suggest that the influence of the anion on the chemical and morphological structure of the hydrothermal carbon has an impact on the activation process. As the impregnation time and carbonization time was kept the same between the samples, it suggests that physicochemical properties that the counter-ion changed had an influence on the ability of H3PO4 to be impregnated into the structure prior to carbonization. Both of the samples that had SO42− ions (H-SO and H-Fe) reported low surface areas, suggesting that although SO42− increases the yield, it is detrimental for H3PO4 activation.
These differences are further highlighted in the pore size distribution date (Fig. 2), where A-Con contains a small distribution of pores between 10–22 Å, A-Cl and A-PO have broader distributions and A-Fe and A-SO have limited porosity development.
Fig. 2 Pore size distribution of the activated materials. Incremental pore volume is displayed via the columns and cumulative pore volume represented by the grey line. |
Overall, the differences in surface area and morphology clearly indicate that the counter ion influences the physicochemical properties of the hydrothermal carbon, which subsequently influences the impact that the activation agent has on the carbon structure. The variation here also indicates that not all ammonium salts are beneficial for creating the high surface area carbon materials required in supercapacitors.
Carbon | Other | |||||||
---|---|---|---|---|---|---|---|---|
CC | C–C, C–Hx | C–OH | –CO | –COOH | –CO3 | Total | ||
H-Con | 23.75 | 28.75 | 17.76 | 7.43 | 2.63 | 1.42 | 81.75 | |
H-SO | 30.67 | 27.35 | 11.61 | 4.66 | 2.15 | 1.18 | 77.62 | 1.11 S |
H-Cl | 27.82 | 31.59 | 8.76 | 4.60 | 2.99 | 1.10 | 76.87 | 0.63 Cl |
H-Fe | 17.35 | 29.05 | 15.77 | 6.88 | 4.36 | 1.44 | 74.83 | 1.17 S |
H-PO | 24.03 | 35.49 | 11.71 | 3.63 | 2.07 | 0.75 | 77.68 | 0.7 P |
Nitrogen | Oxygen | |||||||
---|---|---|---|---|---|---|---|---|
Pyridinic | Amine | Pyrroles | Quaternary | Total | OC | O–C | Total | |
H-Con | 0.00 | 0.00 | 0.00 | 0.00 | 9.92 | 8.36 | 18.28 | |
H-SO | 1.47 | 2.03 | 1.49 | 0.54 | 5.53 | 9.43 | 6.31 | 15.74 |
H-Cl | 0.53 | 0.82 | 1.92 | 0.15 | 3.42 | 12.36 | 6.72 | 19.08 |
H-Fe | 0.46 | 1.24 | 0.70 | 0.52 | 2.92 | 10.74 | 10.33 | 21.07 |
H-PO | 1.47 | 1.86 | 1.45 | 0.38 | 5.16 | 7.21 | 9.24 | 16.45 |
Carbon | Phosphorus | |||||||
---|---|---|---|---|---|---|---|---|
CC | C–C, C–Hx | C–OH | –CO | –COOH | –CO3 | Total | ||
A-Con | 40.35 | 19.52 | 8.09 | 4.64 | 2.77 | 2.96 | 78.35 | 4.15 |
A-SO | 31.68 | 22.20 | 8.07 | 5.49 | 3.39 | 3.37 | 74.2 | 2.7 |
A-Cl | 35.11 | 19.49 | 8.58 | 4.56 | 3.45 | 2.96 | 74.15 | 4.06 |
A-Fe | 36.13 | 17.79 | 9.46 | 3.90 | 3.04 | 2.71 | 73.02 | 4.85 |
A-PO | 42.01 | 12.80 | 9.71 | 3.95 | 3.18 | 3.07 | 74.72 | 3.69 |
Nitrogen | Oxygen | |||||||
---|---|---|---|---|---|---|---|---|
Pyridinic | Amine | Pyrroles | Quaternary | Total | OC | O–C | Total | |
A-Con | 7.32 | 10.19 | 17.5 | |||||
A-SO | 1.45 | 0.85 | 2.24 | 0.77 | 5.31 | 6.38 | 11.23 | 17.79 |
A-Cl | 0.74 | 0.22 | 1.30 | 0.77 | 3.02 | 10.09 | 7.43 | 17.52 |
A-Fe | 1.28 | 0.53 | 1.92 | 0.45 | 4.18 | 8.67 | 9.29 | 17.96 |
A-PO | 0.61 | 0.28 | 1.10 | 0.39 | 2.37 | 12.32 | 6.90 | 19.22 |
The N-doped carbons contained less oxygen surface functionalities than H-Con, a trend that is attributed to the occurrence of Maillard reactions forming various nitrogen groups instead of furans in the hydrothermal reactor.17,28 The type of counter ion also influenced the amount of nitrogen present on the surface. For instance, (NH4)2HPO4 achieved the highest incorporation at 5.16 at% (H-PO), while (NH4)2FeSO4 produced the lowest at 2.92 at% (H-Fe). Additionally, the ratio of nitrogen groups varies based on the counter ion suggesting a nitrogen functionality can be tuned via changing the counter ion. This can be seen by looking at the concentrations of each group between the samples, but is more easily demonstrated if the concentrations are converted into a ratio based on one of the groups. For instance, normalizing to pyridinic groups, the ratio between functionalities in H-SO is 1pyridinic:1.37amine:1.01pyrrolic:0.36quaternary, whereas H-Cl is 1pyridinic:0.67amine:1.60pyrrolic:0.13quaternary. Thus, Cl− produces significantly less amine groups on the surface but a higher number of pyrroles than SO42−. The normalized results for each sample is presented in the ESI† for reference. Sample H-Cl is particularly promising as the formation of amine groups is suppressed compared to pyrroles and pyridinic groups. Amine groups are undesirable for supercapacitors, as these groups are potentially more likely (less energy required) to be cleaved from the surface compared to ring nitrogen, leading to cell degradation under cycling.
Oxygen group distribution was also impacted by the ammonium anion. Normalizing to C–O– groups, H-Con has a ratio of 1C–O–:0.41CO:0.14COO−:0.08CO3 in the C1s peak, whereas H-Cl was 1C–O–:0.52CO:0.32COO−:0.12CO3 and H-PO was 1C–O–:0.31CO:0.17COO−:0.06CO3. Again, Cl− has produced a more theoretically ideal surface, with a lower ratio of cleavable C–O– groups relative to potentially (electrochemically) reversible CO functionalities.50
Duel heteroatom doping has also occurred, with the counter ion being incorporated into the structure in H-SO (1.11 at% S), H-Cl (0.63 at% Cl), H-Fe (1.17 at% S) and H-PO (0.7 at% P). Despite (NH4)2HFeSO4 containing three potential dopants (N, S and Fe), only N and S were detected on the surface of H-Fe. This was unexpected, as Fe has been previously incorporated hydrothermally using Fe(NO3)3·9H2O.51 However, that study incorporated a series of pre-treatment steps that were not performed here, such as soaking in a Fe(NO3)3·9H2O solution and pH adjustment, which might be critical for Fe incorporation into hydrothermal carbon.
The XPS results indicate that changing the counter ion has a substantial influence on the surface functionality and can provide another method to tune the surface of hydrothermal carbon for various applications. However, the tunability provided from the counter ion may be less important if the tuning is not carried out after activation. Fortunately, activation with H3PO4 actually enhances the benefits already provided from using different anions. For instance, the ratio of nitrogen groups in A-Cl is 1:0.29:1.75:1.03 (H-Cl is 1:0.67:1.59:0.13) for pyridinic, amine, pyrrolic and quaternarty, indicating an increase in the ratio of benificial pyrrolic, pyridinic and quaternary nitrogen groups during activation. Amine groups are reduced in all of the samples during activation, leaving a distribution of quaternary, pyrrolic and pyridinic functionalities. The activation step also incorporated between 2.7 to 4.85 at% phosphorus onto the surface, leaving the surface with oxygen, nitrogen and phosphorus functionalities.
While XPS is a robust method for quantifying elemental concentration on carbon surfaces, deconvolution is necessary to obtain quantitative information about the functional groups associated with each elemental peak. This can be problematic when a single broad peak is obtained that overlaps several functional group regions,38 making it unclear if the peak represents a single functionality or multiple functional groups. Thus, a secondary technique is required to confirm the presence of these functional groups. FTIR is commonly utilized for this reason, however nitrogen and oxygen functional groups can be difficult to differentiate with FTIR. Therefore we have used carbon K-edge and nitrogen K-edge NEXAFS to confirm the functionalities indicated by XPS and probe the surface of these materials further.
The carbon K-edge contains two easily observable differences between H-Con and the nitrogenated hydrothermal carbons (Fig. 3(a)) at 286.5 eV and 288.5 eV. The peak at 286.5 eV is associated with the furanic structure of hydrothermal carbon and its intensity decreases in the nitrogenated materials. Previous work established that nitrogen reduces the number of furan structures in the hydrothermal carbon structure, reducing the intensity of the peak at 286.5 eV.17 The same effect is clearly being replicated here with each ammonium salt.
Fig. 3 NEXAFS carbon K-edge spectra of (a) hydrothermal carbons (H-) and (b) activated hydrothermal carbons (A-). Functional group locations for the main C1s → π* and C1s → σ* are added for reference and based on previous NEXAFS work on hydrothermal carbons.17 The long dashed lines represent the position of the arctangent step function at 290.0 eV. |
The second difference at 288.5 eV, associated with C1s → π* transitions on COOH, COamides, and CCpyrroles,52 displays an observable increase in intensity for all of the nitrogenated carbons compared to H-Con. As the concentration of COOH groups does not vary significantly in the XPS, the increased peak height at 288.5 eV is attributed to the presence of amides and pyrroles. These groups can also be observed in the nitrogen K-edge spectra (Fig. 4) at 401.3 eV, confirming their presence. Overall, the carbon K-edge indicates that the hydrothermal N-doped materials have a similar carbon structure with variations in the concentration of functional groups, further demonstrating that tuning the surface functionality is possible through changing the anion.
Fig. 4 NEXAFS nitrogen K-edge spectra of (a) hydrothermal carbons and (b) activated hydrothermal carbons. Functional group locations for the main N1s → π* and N1s → σ* are added for reference and based on previous NEXAFS work on hydrothermal carbons.17 The long dashed lines represent the position of the arctangent step function at 403.9 eV and 406.5 eV. |
After activation with H3PO4, the sharp peaks associated with oxygen/nitrogen functionalities between 286.5 to 290 eV are almost completely removed, while peaks associated with aromatic groups increase. The loss of oxygen functionality and increased aromatic concentration after activation is a common occurrence, which is escalated with increasing temperature.42 What is interesting is the peak at 288.5 eV (COOH, COamides, and CCpyrroles52) is still present in the N-doped carbons, but not in A-Con. This suggests that pyrroles have survived the activation process, as they are also observed in the nitrogen K-edge spectra (Fig. 4) at 401.3 eV.
In addition to pyrrolic groups (401.3 eV), the nitrogen K-edge spectra also indicates the presence of pyridinic groups (399 eV). The first peak at 399 eV exclusively occurs from CN N1s → π* transitions on pyridinic groups, whereas the second peak is related to a combination of N1s → π* transitions on imine (401.3 eV), amide (401.3 eV) and pyrrolic groups (401.9 eV). In H-PO a third peak can be also observed at 402.9 eV, related to unsaturated NCpyrrolic structures.
The influence of the counter ion is again displayed here, with a clear difference in peak heights for the pyridinic groups at 399 eV (PO43− > SO42− > Cl− > Fe2+ + SO42−) and pyrrolic groups at 401.3 eV (Cl− > SO42− > PO43− > Fe2+ + SO42−). The differences in intensity here between the samples match the concentration differences in the XPS results.
The intensity of the nitrogen peaks decreased after activation, indicative of nitrogen loss, although the degree of nitrogen loss was not equally shared across all nitrogen functionalities. Pyridinic groups, especially in A-PO and A-SO, lost considerable intensity after activation, compared to pyrroles. This difference could stem from the weakly basic nature of pyridine, which would have accepted a proton from H3PO4 and increased its reactivity. From a previous study pyridinic groups appeared to also be impacted more by temperature than pyrrolic.42 This loss was further escalated when H3PO4 was used as an activation agent.
A-Cl provided the highest capacitance and cycle stability (194.7 F g−1), followed by A-Con (155.4 F g−1), A-Fe (89.8 F g−1) and A-SO (67.7 F g−1). The results for A-Cl and A-Con are in the same range of a study by Misnon et al. using 1 M KOH, where they achieved from 110 to 210 F g−1 for their activated carbon from oil palm kernel.54 Apart from A-PO which has a clearly unstable surface characteristics, it is difficult to see the influence of the counter ion or nitrogen in a CV as the capacitance stored in the electrical double later is so large. Thus, SPECS was employed to break down the different capacitance contributions.
The advantage of the SPECS method is that a synthetic voltammogram for each charge storage mechanism can be generated, since the current response for each potential step has been deconvoluted into its individual components.43,44Fig. 7(a) and (b) show the synthetic voltammograms for A-Con sample at the cycle rates of 5 and 50 mV s−1 respectively. As expected, the average current increases with an increasing sweep rate. It can be seen that the synthetic voltammogram for the capacitive current at the porous surface area is greater than the capacitive current at the geometric surface area at the low sweep rate of 5 mV s−1, as at lower sweep rate there is more time for ions to cover the surface of inner pores. While at higher sweep rate the contribution of geometric capacitive process (DL1surface) is greater than the capacitive process at the porous surface area (DL2pores). Fig. 7(a) and (b) also indicate that overall the capacitive processes are the dominant charge storage mechanisms and diffusion limited processes have a slight contribution in charge storage mechanisms. This is due to the nature of carbon-based electrode materials, which mainly store charge through the capacitive processes. The origin of the diffusion limited processes in carbon-based electrodes is from diffusion into restrictive pores.
Fig. 7 Synthetic voltammogram obtained from the SPECS data for A-H, comparing behavior at different sweep rates of (a) 5 mV s−1 and (b) 50 mV s−1. |
The synthetic voltammograms generated from the SPECS analysis can also be used to determine the specific capacitance as a function of cycle rate. The added benefit here is that because the SPECS data was deconvoluted into individual processes, from which the contributions made by each process to the overall voltammogram have been calculated, the capacitance of the individual processes can be calculated vs cycle rate. Fig. 8 shows the total specific capacitance and the specific capacitance of the geometric (DL1surface), porous (DL2pores) surfaces, the diffusion limited capacitance, and the residual capacitance, obtained from the SPECS data as a function of the sweep rate. A-PO has not been included in the SPECS analysis as the material was unstable under cycling.
In all four samples, DL1surface displays limited change at different cycle rates, due to being associated with the geometric surface area and thus has no ion transport limitations. The higher capacitance for DL1surface in A-Con and A-Cl is likely due to having a higher geometric surface area for the material. The contribution from DL2pores follows the specific surface area, with higher surface areas producing a larger contribution from DL2pores, simply due to having higher total pore volume. However, it is important to consider the pore size distribution (Fig. 2) and how that impacts on the capacitance contribution from DL2pores and the diffusion limited capacitance.
The bare ion radii of K+ is 1.33 Å (d = 2.66 Å) and the solvated ion radii is 3.31 Å (d = 6.62 Å),55 therefore only a single solvated ion will fit in the pores between 3 to 6 Å. Considering that the SPECS experiments were performed in an aqueous electrolyte, it is likely that all of the ions are in their solvated state, unlike in organic and ionic liquids where desolvated ions are more common because of their weaker polarity (solvent) and charge density (ions). Despite the solvated ion fitting into these smaller pores, this restrictive environment reduces the likelihood that an ion will be pushed into these pores. Thus, only at lower cycle rates when there is sufficient time for an ion to travel down these pores do they become active. This is the reason why DL2pores starts to plateau at lower sweep rates, as the double layer is accessing the maximum surface area available to it at this point. It is also at this point that diffusion limited capacitance starts to increase significantly, as it represents the mass transport of ions into increasingly smaller pores. The higher level of diffusion and lower DL2pores in A-Con compared to A-Cl is directly related to its porosity, with almost 65% of the porosity in A-Con located in pores smaller than 15 Å, compared to A-Cl where only 44% is located in this region. This is further demonstrated when examining the ratio between the capacitance contributions of DL1surface and DL2pores for A-Con and A-Cl. As DL1surface is almost identical in A-Con and A-Cl, we can consider that the geometric surface is similar in both materials, however in A-Con the capacitance from DL2pores is about 1.5 times higher at 50 mV s−1, whereas it is 3.3 times higher in A-Cl at 50 mV s−1. Even at lower sweep rates, where smaller pores will become accessible, A-Cl still has a higher ratio (5.0 at 5 mV s−1) than A-Con (3.2 at 5 mV s−1). Thus, the surface of A-Cl is far more accessible than A-Con.
The residual current and diffusion are higher in A-Con compared to the nitrogen doped materials, suggesting that this surface is a lot more electrochemically active at slower scan rates. The residual represents kinetically slow redox processes that are ongoing beyond the duration of each potential step. These processes or electrode instabilities become apparent after the electrode is left to rest at a fixed potential for an extended period of time. Thus, the residual can be considered to be similar to a floating test across the full potential window. Thus, the combination of a more electrochemically active surface (higher residual) and restricted pores (higher diffusion) results in the total performance of A-Con being higher at cycle rates <1 mV s−1 than the nitrogen doped materials. However, if the residual current is not zero, then there are potential stability issues with the system. Thus, A-Con is likely to fail earlier than A-Cl due to these instabilities in the electrode surface.
Examining whether the incorporation of nitrogen into these materials has enhanced their performance is difficult, as the surface area and porosity is vastly different between each of the ammonium salt added materials and the control. What is observed here is that the ammonium counter ion has an influence on the hydrothermal reaction, which subsequently influences the ability for the hydrothermal carbon to increase its surface area under activation and these impacts are displayed in the electrochemistry. However, it is interesting that again we have a nitrogen doped material that does not display clear redox peaks in the CV, which seemingly contradicts the literature which continuously states that nitrogen introduces pseudocapacitance through redox active sites. In fact studies examining nitrogen doped carbon materials don’t appear to display any clear redox behaviour in their cyclic voltammetry data,16,20,56 unlike the electrochemical redox behaviour of the quinone group which is easily observable.57 What might be occurring here is that nitrogen is providing a localised charge storage site on the surface of the material, which is electrically connected to the carbon and the electrical double layer. Thus, a specific redox peak will not be observable. Additionally, the benefit of nitrogen may come from its other suggested properties, such as wettability,5 electrode stability and lower resistance.7
To examine if nitrogen doping does indeed have an impact on the resistance, electrochemical impedance spectroscopy (EIS) was used to examine A-S, A-SO, A-Cl and A-Fe with the Nyquist plot presented in Fig. 9. Each of the samples displayed the typical shape of a semicircle followed by a tail. Instead of fitting each of the EIS to RC circuits, a physical interpretation of the plot was performed based on the examination of EIS for supercapacitors by Mei et al.58 The electrode resistance is represented as the distance between 0 and the first data point on the Re(Z) axis and the bulk electrolyte resistance is represented as the diameter of the semicircle. The sum of these two properties represents the internal resistance of the electrode. Calculating the internal resistance resulted in the nitrogenated materials having a slightly lower resistance (A-SO 13.77 Ω, A-Cl 15.72 Ω, A-Fe 14.01 Ω) than A-Con (16.82 Ω), indicating that the suggestion that nitrogen improves conductivity is likely to be valid here as well.
These benefits could be the reason why the residual current is far lower in the nitrogen doped materials compared to A-Con, as the incorporation of nitrogen creates a more stable electrochemical surface. Overall, further examination of how nitrogen contributes to capacitance through the examination of pseudocapacitance, conductivity, wettability and electrochemical testing is needed to understand its impact.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d0ma00601g |