Department of Chemistry, Indian Institute of Technology Hyderabad, Kandi, 502285, Sangareddy, Telangana, India. E-mail: mdeepa@chy.iith.ac.in
First published on 4th May 2020
Efficient storage of sunlight in the form of charge is accomplished by designing and implementing a photo-supercapacitor (PSC) with a novel, cost-effective architecture. Sulfur (S)- and nitrogen (N)-doped graphene particles (SNGPs) are incorporated in a TiO2/CdS photoanode. The beneficial effects of SNGPs such as the high electrical conductance promoting fast electron transfer to TiO2, a suitably positioned conduction band that maximizes charge separation, and its' ability to absorb red photons translate into a power conversion efficiency of 9.4%, for the champion cell. A new composite of poly(3,4-propylenedioxythiophene)/carbon micro-sphere-bismuth nanoflakes (PProDOT/CMS-BiNF) is integrated with the photoanode to yield the PSC. The photocurrent produced under 1 sun irradiance is directed to the supercapacitor, wherein, the synergy between the faradaic and electrical double layer charge accumulation mechanisms of PProDOT and CMS-BiNF bestows storage parameters of an areal capacitance of 104.6 mF cm−2, and energy and power densities of 9 μW h cm−2 and 0.026 mW cm−2. An overall photo-conversion and storage efficiency of 6.8% and an energy storage efficiency of 72% exhibited by the PSC are much superior to those delivered by a majority of the PSCs reported in the literature on the otherwise highly efficient perovskite solar cell or the expensive Ru dye based solar cells.
Digressing from these popular choices for the PV and storage components, in this report, an inorganic semiconducting chalcogenide and doped graphene particles are used as co-sensitizers in the solar cell part. Graphene quantum dots (GQDs) as green photosensitizers in photovoltaic,14 photocatalysis15 and supercapacitor16 applications are an exciting class of materials, for they are non-toxic, environment friendly, are capable of absorbing a broad spectral range, are chemically stable, offer high carrier mobility and tunable band gaps. Furthermore, by replacing some of the carbon atoms with hetero atoms like S and N in the graphitic lattice, more defect states are introduced, which modifies the electronic structure of graphene, and thus alters its' electrical, optical and physicochemical properties.17,18 Relying on this approach, in this study, sulfur (S) and nitrogen (N) doped graphene particles, labeled as SNGPs, were synthesized by a hydrothermal route, and anchored to the TiO2 support, followed by CdS deposition to yield the high performing TiO2/SNGP/CdS photoanode. A literature survey also confirms the ability of GQDs to serve as efficient photoactive materials.19,20
Besides the photoanode, the counter electrode (CE) of the solar cell also controls the PV response. An ideal CE should be electrically conducting and have a high surface area to bring about the electrocatalytic reduction of the oxidized species in the polysulfide/silica gel electrolyte. Conducting polymers (CPs), carbon nanomaterials, metal nanoparticles and their composites have been explored as CEs in solar cells,21,22 and also as electroactive electrodes in supercapacitors.23,24 Of the lesser studied conducting polymers is poly(3,4-propylenedioxythiophene) or PProDOT.25 Lee et al.25 used PProDOT-Et2, PProDOT, PEDOT, and sputtered-Pt electrodes as CEs in dye sensitized solar cells (DSSCs) which showed PCEs of 7.88, 7.08, 3.93 and 7.77% respectively. PProDOT based cells were characterized by PCEs comparable to that achieved with a Pt CE, whereas with PEDOT, a lower PCE was obtained. Ahmad et al.26 prepared nanoporous layers of PProDOT with three different ionic liquids and used them as CEs, and the PProDOT with the most hydrophobic ionic liquid dopant displayed good catalytic properties to result in a PCE > 9%, which was significantly higher than the other Pt free CEs. A composite CE of PEDOT/multiwalled CNTs in a Ru dye based DSSC showed a PCE, greater by 13% than the DSSC with a PEDOT CE. The higher PCE was ascribed to low charge transfer resistance at the PEDOT/MWCNT/electrolyte interface and high electrocatalytic activity for the reversible I3−/I− redox reaction.27 Rafique et al.28 reported an Ag-PPy-functionalized MWCNT nanocomposite CE based DSSC, which delivered a PCE of 7.6%, higher than that obtained with a traditional Pt CE.
Other aspects of PProDOT such as fast redox switching and a lower oxidation potential than PEDOT etc. also validate its use in a supercapacitor.29 However, during repeated charge–discharge cycling, the polymers suffer from swelling and shrinkage due to counter ion doping and de-doping, which imparts mechanical stress and can accelerate its' delamination from the current collector. Use of composites with carbons, can help in improving cycling life, for the carbon nanomaterial can buffer the volume change experienced by the polymer, also increase the mechanical strength of the electrode.30 To this end, in a previous study, a PEDOT/graphene oxide (GO) composite based supercapacitor31 showed a SC of ∼115 F g−1 and an energy density of 13.6 W h kg−1 at a current density 0.3 A g−1, significantly improved relative to the pristine polymer's storage properties, and assigned to the high surface area of GO that amplifies the faradaic reaction of the polymer. PProDOT/single-walled CNT (SWNTs), helically wrapped with conjugate poly[2,6-{1,5-bis(3-propoxysulfonicacidsodiumsalt)}naphthylene]ethynylene exhibited a 90% SC retention after 21000 cycles, compared to PProDOT, which retained only 84% of its' initial SC.32 Nanocomposites of Ag/MnO2/RGO showed a much higher SC of 467.5 F g−1 compared to MnO2/RGO electrode (293.2 F g−1). In this ternary nanocomposite, Ag nanoparticles improved the electrical conductivity and promoted electron transfer.33
Based on this background, a configuration with TiO2/SNGP/CdS as the photoanode, and a new composite of PProDOT with carbon micro-spheres (CMS), and bismuth (Bi) nanoflakes (BiNF) as the CE as well as the energy storage electrode is proposed for a PSC. Through elaborate structural details coupled with optical, electrochemical and photoelectrochemical studies, the rationale for developing this PSC with a unique configuration and the potential it has for practical applications is illustrated.
A polysulfide gel electrolyte is used in the solar cell and it was prepared by dispersing 5 wt% of silica powder in an aqueous solution of 1 M Na2S and 1 M S, with continuous stirring in a beaker at room temperature. The yellow colored homogeneous, slightly turbid gel was poured into a cavity created by a parafilm spacer over the CE: PProDOT/CMS-BiNF film over the long Ni foam substrate. The TiO2/SNGP/CdS electrode was placed with the film side facing inwards over the gel, to yield the solar cell part. For the supercapacitor part, a lithium ion conducting gel polymeric electrolyte was synthesized by dissolving PMMA (0.7 g) in the clear 1 M LiClO4/PC (1 g in 10 mL) solution. After vigorous stirring at 80 °C for 8 h, a colorless transparent gel was obtained and it was cooled to ambient temperature. This gel was applied over a GF/D spacer, which was sandwiched between the two electrodes of the supercapacitor part of the PSC, placed over the PProDOT/CMS-BiNF@Ni foam end. Another PProDOT/CMS-BiNF electrode fabricated separately was affixed over the supercapacitor part of the cell (Scheme 2). The labels (A), (B) and (C) in Scheme 2 are the three points for taking electrical connections for operating the PSC. The PSC cell was exposed from the rear side for all experiments involving irradiance. For all electrochemical and photoelectrochemical measurements, a minimum of five electrodes of a given composition were tested.
The electrolytes used for both parts: the photovoltaic part, and the symmetric supercapacitor part are gels, which are highly viscous, and did not exhibit any visible sign of leakage, over long term operation. Leakage usually occurs if the gel is used in excess, the amount is optimized to prevent the oozing out of the gel. The gel used for the symmetric supercapacitor part has PMMA as the gelatinizing agent. PC is a non-volatile solvent with a high boiling point of 240 °C, and therefore this gel does not evaporate during operation. Further the gel is not only applied over the electrodes, but is also applied over a GF/D spacer which is 1.2 mm thick and has pores of ∼2.7 μm dimensions, and therefore, once the gel penetrates through the cross-section of the separator, its' proportion is ample for long term use. For the solar cell part, a polysulfide/silica gel electrolyte was used, where fumed silica assists in the formation of a quasi-solid state electrolyte and also restricts the photo-corrosion of the QDs. The spacer has a thickness of 2 mm, which allows a sufficient amount of gel to be incorporated between the two electrodes. Since this gel is not exposed, there is no distinct evaporation.
Bi nanoflakes, appear as large florets made up of discrete flakes (Fig. 1f), and the inter-flake gaps can potentially serve as active centers for electron transfer during the solar conversion, and as sites for accepting ions, during charge–discharge of the supercapacitor. The corresponding lattice scale image shows the flakes to be highly crystalline, having parallely oriented lattice fringes with an inter-fringe distance of 3.26 Å (Fig. 1g). This separation matches with an interplanar “d” spacing of 3.26 Å of the rhombohedral crystal lattice of Bi (PDF no: 85-1331). It is assigned to the (012) plane of Bi. An XRD pattern of Bi nanoflakes confirms the same, for it displays multiple peaks at 2θ of 22.6°, 27.2°, 38.1°, 39.7°, 44.7°, 46.1°, 48.8°, 56.2°, 62.5° and 64.7° with d-spacings of 3.93, 3.26, 2.35, 2.26, 2.02, 1.96, 1.86, 1.63, 1.48 and 1.43 Å, aligning with the (003), (012), (104), (110), (015), (006), (202), (024), (116) and (122) planes of the rhombohedral structure of Bi (Fig. 1h).35 The XRD pattern of PProDOT shows three broad humps at 2θ of 24.4°, 44.2 and 62.5°. The most intense hump is close to the (002) plane of graphitic carbon (PDF: 74-2330) with d = 3.6 Å (Fig. 1i). It is ascribed to the intermolecular π–π* stacking of the polythiophene rings.34 Carbon micro-spheres show peaks at 2θ of 26.1°, 43.4° and 54.1° with d values 3.4, 2.1, and 1.7 Å corresponding to the (002), (101) and (004) planes of hexagonal graphite (PDF: 75-1621) (Fig. 1j). Fig. 1k and l show the Raman spectra of PProDOT and carbon micro-spheres. PProDOT exhibits five prominent peaks at 1100, 1265, 1417, 1485 and 1548 cm−1, attributed to the bending mode of the C–O–C group in the propylenedioxy ring, intermolecular Cα–Cα′ inter-ring stretching mode, symmetric CαCβ(–O) stretching vibration on the 5-membered ring, and symmetric and asymmetric intra-ring CαCβ vibrations.34 Carbon micro-spheres produce two distinct peaks at 1360 (D-band) and 1599 (G-band) cm−1 corresponding to disordered carbon and in-plane bond stretching of the sp2 hybridized carbon atoms as in graphitic carbon.36
Fig. 2e shows the full scan XPS spectrum of SNGPs in which the peaks at 532, 400.2, 284.5, 228 and 164.6 eV, are assigned to the O1s, N1s, C1s, S2s and S2p signatures respectively, revealing the doping of S- and N- on graphene particles.37 A deconvoluted C1s spectrum exhibits three components at 284.6 and 285.3 and 288.5 eV attributed to the C–C, (C–N/C–S/C–O) and CO bonds respectively (Fig. 2f). The N1s spectrum is resolved into three peaks at 398.9, 400.5 and 401.7 eV which originate from the pyridinic, pyrrolic and graphitic – type nitrogen in the carbon framework (Fig. 2g). An S2p spectrum is resolved into three peaks at 163.7, 164.6 and 168.7 eV and while the former two represent the spin–orbit split components of S2p3/2 and S2p1/2 with a peak separation of 4 eV and an intensity ratio of 2:1, the latter peak stems from an oxidized sulfur group (Fig. 2h). Thus, the presence of nitrogen and sulfur in the graphene particles is confirmed. The electrical conduction capability of SNGPs is affirmed from linear sweep voltammetry, performed using a two probe system. On a clean glass substrate, SNGP solution was drop-cast and heated for 3 h at 80 °C. Two “SS all pins” were positioned vertically with their tips gently contacting the surface of the SNGP film without puncturing the same and then connected to a potentiostat. I–V measurements were done over a voltage range of −0.3 to 0.3 V, and from the linear fit, the conductance of SNGPs is determined by employing the relation: ΔI/ΔV = 1/R = slope (G) and it is 1.1 mS (Fig. 2i). This conductance is sufficient for channelizing the photo-excited electrons from CdS to TiO2, thereby suppressing back electron transfer to the oxidized polysulfide species in the electrolyte at the TiO2/SNGP/CdS/Sn2− interface in the solar cell part of the PSC, during the PSC operation.
To assess the excited state electron transfer and propagation in the TiO2/SNGP/CdS photoanode, fluorescence spectra of pristine CdS, SNGPs and their composite photoanodes, were recorded and are displayed in Fig. 3c and d. SNGPs, when excited at λex of 370 nm, yields three emission peaks with λmax positioned at 433, 515 and 633 nm. Possible transitions due to the different chromophores present in SNGPs, in the form of CO, C–S, C–N covalent linkages, could be the reasons for the multiple bands. CdS produces a broad emission over the 500–600 nm span with a λmax at 534 nm; it is assigned to the band edge recombination. Transitions between the intra-gap trap states induces the broadness.39 The SNGP/CdS composite has a fluorescence profile resembling that of CdS, but has a lowered overall intensity by about 28%. TiO2/CdS and TiO2/SNGP/CdS photoanodes show quenched emission bands, with intensities reduced by 47.7% and 69% relative to CdS. SNGPs produce a distinct band in the 600–700 nm range, which is not observed in TiO2/CdS. This quenching is attributed to the transfer of photo-generated electrons from the conduction band (CB) of CdS to the CB of TiO2via SNGPs (if present) through the cascade mechanism process. It is also observed that the SNGP's fluorescence peak with a λmax at 433 nm is completely quenched in both SNGP/CdS and TiO2/SNGP/CdS, indicating transfer of photo-generated electrons from SNGPs to FTO and TiO2 respectively.
Fig. 3e shows the time-correlated single photon counting (TCSPC) measurements for the photoactive electrodes at excitation and emission wavelengths of 370 nm and 530 nm. Here, a bi-exponential function is used for fitting the parameters. The fitted parameters are given in Table S1 (ESI†). The average lifetimes for photoanodes are evaluated by using the equation given below,
I = B1exp(−t/τ1) + B2exp(−t/τ2). | (1) |
Thus, the electron lifetime is calculated using the equation,
〈τ〉 = ΣBiτi2/ΣBiτi. | (2) |
In eqn (1) and (2), I is the normalised emission intensity, τ1 and τ2 are the electron lifetime decay constants, B1 and B2 are the amplitude coefficients and τ is the average electron lifetime. The average lifetime for CdS of 17.2 ns, is reduced to 9 and 6.1 ns respectively for FTO/SNGP/CdS and TiO2/CdS electrodes. Charge injection from the CB of CdS to the CB of SNGPs and subsequently to FTO in the former and from CdS to TiO2 in the latter are energetically favorable processes, and occur spontaneously when impinged by a monochromatic radiation. Average lifetime for the ternary photoanode of TiO2/SNGP/CdS, further drops to 1.7 ns, affirming efficient charge relay from CdS to SNGP to TiO2. This reduced lifetime also implies that back electron transfer to the electrolyte will be minimized for this co-sensitized photoanode, compared to TiO2/CdS, when used in a solar cell. An energy band diagram illustrating the positions of CBs and valence bands (VBs) of TiO2, SNGPs and CdS and the direction of charge transfer can be seen in Fig. 3f. Cyclic voltammetry (CV) plots (Fig. S1, ESI†) were used to determine the CBs and by subtracting the optical Eg from the CB, the VBs were estimated. The values of CB, Eg and VB are summarized in Table S2 (ESI†). Upon excitation, in the TiO2/SNGP/CdS photoanode, while hole transfer is thermodynamically feasible from the VB of CdS to the S2− species in the electrolyte, the VB positions of CdS and SNGPs do not permit the same. However, since we obtained a superior PCE for TiO2/SNGP/CdS (9.4%) compared to TiO2/CdS (7.7%) and TiO2/SNGP (1.7%) based solar cells, and a finite PCE of 0.6% for the FTO/SNGP/CdS cell as well (Fig. S2†); we conclude that the Fermi level or the intra-gap trap states which are positioned above the VB in CdS, allow for hole transfer, thus completing the circuit, and leading to the high efficiency.
Solar cell configuration | J SC (mA cm−2) | V OC (V) | FF | η (%) | η average (%) |
---|---|---|---|---|---|
TiO2/CdS–Ni | 11.82 | 0.676 | 0.41 | 3.33 | 3.29 ± 0.03 |
TiO2/CdS–PP@Ni | 13.84 | 0.736 | 0.54 | 5.47 | 5.40 ± 0.06 |
TiO2/CdS–PP/CMS@Ni | 14.56 | 0.783 | 0.59 | 6.72 | 6.64 ± 0.05 |
TiO2/CdS–PP/CMS-BiNF@Ni | 15.40 | 0.807 | 0.63 | 7.83 | 7.74 ± 0.08 |
TiO2/SNGP/CdS–Ni | 16.08 | 0.685 | 0.41 | 4.53 | 4.50 ± 0.03 |
TiO2/SNGP/CdS–PP@Ni | 17.07 | 0.740 | 0.56 | 7.10 | 7.08 ± 0.04 |
TiO2/SNGP/CdS–PP/CMS@Ni | 17.61 | 0.790 | 0.60 | 8.42 | 8.34 ± 0.06 |
TiO2/SNGP/CdS–PP/CMS-BiNF@Ni | 18.2 | 0.822 | 0.63 | 9.50 | 9.41 ± 0.06 |
TiO2/SNGP–PP/CMS-BiNF@Ni | 7.05 | 0.606 | 0.41 | 1.77 | 1.72 ± 0.03 |
The PCE difference from bare Ni foam to the PProDOT/CMS-BiNF composite reveals that the PProDOT/CMS-BiNF offers a low charge transfer resistance at the CE/electrolyte interface, allowing unhindered electron injection to the Sn2− species in the electrolyte and also furnishes a high electrocatalytic activity for the reduction of Sn2− species, thereby maximizing the overall charge separation, and resulting in the highest efficiencies, when combined with a given photoanode. PProDOT and CMS are electroactive materials, where PProDOT can conduct both ions and electrons via doping and de-doping, and CMS spheres can conduct electrons through the conjugated carbon framework. Bi nanoflakes improve the overall electroactivity of this electrode, by providing more number of active sites for electron accumulation. Together, the PProDOT/CMS-BiNF electrode is capable of transferring electrons rapidly to the electrolyte. The champion cell of the TiO2/SNGP/CdS photoanode with the PProDOT/CMS-BiNF composite CE achieves the highest PCE of 9.4% with JSC of 18.2 mA cm−2, VOC of 822 mV and an FF of 0.63 respectively. The synergy between (1) the co-sensitization effect of SNGPs and CdS, which results in broader solar spectrum absorption and conversion at the TiO2/SNGP/CdS photoanode and (2) the high electrocatalytic activity of the PProDOT/CMS-BiNF composite CE comes to the fore in the TiO2/SNGP/CdS–Sn2−/nS2−–PProDOT/CMS-BiNF solar cell, and is responsible for the highest PCE delivered by this cell, in this work.
The role of SNGPs to serve as an independent photosensitizer was evaluated by recording the J–V response of a TiO2/SNGP-Sn2−/nS2−–PProDOT/CMS-BiNF solar cell under 1 sun and in the dark (Fig. 4c). The cell delivers a PCE of 1.77% with a JSC of 7 mA cm−2, VOC of 606 mV and an FF of 0.41 respectively, confirming the ability of SNGPs to function as a material capable of undergoing charge separation upon irradiance. In the dark, the same cell delivered a PCE of 0.07%, which is insignificant compared to the performance under illuminance. We have compared our data with solar cells based on graphene QDs, and also with solar cells based on conducting polymers (CPs) and metal nanoparticle/CP composites and we find that the PCE of 9.4% reported herein for the best cell with an average η of 9.4 ± 0.06%, is significantly enhanced compared to the reported PCEs, which are in the range of 0.6 to 8%.40–44
Metal sulfides are prone to irradiance induced photo-corrosion. The fumed silica in the S/S2− gel electrolyte inhibits the photo-corrosion of CdS and leakage of the polysulfide electrolyte. It serves as a nano-filler for solidifying the electrolyte and enhancing the mechanical strength. The –OH on SiO2 groups have a propensity to bind electrostatically to Cd2+, and thus prevent hole injection to any dissolved oxygen in the electrolyte, which is one of the principal mechanisms for photo-corrosion, as shown in Fig. S3a (ESI†). Excess of photo-generated holes at the CdS surface, which are not consumed by the electron donors, i.e., the S2− species in the electrolyte, are susceptible to reacting with oxygen, resulting in the formation of CdSO4.45 SiO2 effectively reduces this photo-dissolution of CdS. SiO2 also offers an energy barrier for the recombination between photo-generated electrons from the QDs and the oxidized Sn2− species as well as for the recombination between the electrolyte and the injected electrons from TiO2.46 Furthermore, reduced graphene oxide (RGO) has also been shown to inhibit the photo-corrosion of CdS in a photocatalytic system.47 Here too, the vicinal SNGPs provide suitably aligned energy states for the rapid extraction of the photo-excited electrons from CdS.
The stability tests for the cell with the following configuration: TiO2/SNGP/CdS-polysulfide/silica gel-PProDOT/CMS-BiNF and the variation of photovoltaic parameters as a function of illumination time (to 1 sun or 100 mW cm−2) are shown in Fig. S3b (ESI†). J–V characteristics of this cell were measured at every 2 h interval and the solar cell parameters are given in Table S4.† When the cell was measured for the first time, the PCE was 9.4% with JSC of 18.16 mA cm−2, VOC of 0.81 V and an FF of 0.63 respectively. After 10 h, it still gave a PCE of 8.82%, which is lowered by ∼6.2% compared to the initial value. In the past, for a QDSC with a TiO2/CdS/CdSe/polysulfide/PbS-carbon black configuration, the PCE decreased from 3 to 2.7% after 1000 h of illumination, which corresponds to a 10% loss in PCE.48 In another study of a TiO2/CdS/CdSe based cell with a CuS CE, the initial PCE of 4.22% decreased to 4.0% after 2 h of continuous illumination.49 A cell with a TiO2/CdSeS–ZnS photoanode and a Pt CE showed an initial PCE of 4.23% and, after 8 h of irradiation, it decreased to 2.32%, thus amounting to a loss in PCE by ∼45%.50 The cell fabricated in this study is also able to endure prolonged exposure without undergoing significant deterioration, indicating the role of fumed silica particles, and SNGPs in imparting an acceptable stability to the system.
Nyquist plots for the cells with TiO2/CdS and TiO2/SNGP/CdS photoanodes and having the same CE of the PProDOT/CMS-BiNF CE with the polysulfide/silica gel electrolyte (Fig. 4d), further demystify the role of SNGPs. The measurements were executed in the dark over a frequency range from 0.1 Hz to 1 MHz having an ac amplitude of 20 mV and at an open circuit voltage of 0.8 V. Two semicircles are obtained for both cells, and the data was fitted into an electrochemical circuit of [Rb(RCE × QCE)(Rrec × Qrec)] and these parameters are given in Table S5 (ESI†). Rb is assigned to the bulk resistance of the gel, RCE and QCE are the resistance and corresponding constant phase elements at the CE/electrolyte interface, and Rrec and Qrec are the resistance and corresponding constant phase elements at the photoanode/electrolyte interface. Rb for TiO2/CdS and TiO2/SNGP/CdS are 20.7 and 22.2 Ω cm2 respectively which are almost equal. The TiO2/CdS cell shows a lower recombination resistance (Rrec) of 11.5 Ω cm2 than the same cell co-sensitized with SNGPs (21.6 Ω cm2). Thus, electron–hole recombination is reduced at the TiO2/CdS photoanode/polysulfide electrolyte interface when SNGPs are sandwiched between TiO2 and CdS and results in significant improvement in the PCE. It is also reflected in the Bode phase plot (phase angle versus frequency) (Fig. S4, ESI†). The electron recombination time (τn) is determined by using the formula, τn = 1/2πfmax, where fmax is the peak frequency. Thus, τn for TiO2/CdS and TiO2/SNGP/CdS photoanodes are 1.1 ms and 1.6 ms respectively. It reveals the role of TiO2/SNGP/CdS in reducing the recombination with oxidized species of the polysulfide electrolyte.
The electrocatalytic activity of Bi nanoflakes in the CE was verified from an LSV plot and a Nyquist plot shown in Fig. S5 (ESI†). Ni foam and BiNF@Ni show reduction potentials peak at −0.59 and −0.56 V respectively, indicating that while the overpotential is 0 V with blank Ni, the reduction potential required for this reduction is slightly lowered with BiNF. Similarly, Nyquist plots were compared for the Ni//Ni and the Ni@BiNF//BiNF@Ni symmetric cells, again with the polysulfide electrolyte over a frequency range of 1 MHz to 0.1 Hz. Two skewed semicircles are observed for the two cells based on Ni and Ni@BiNF. Here, BiNF@Ni shows a lower charge transfer resistance (14.6 Ω cm2) compared to Ni alone (19.2 Ω cm2). Thus, BiNF exhibits superior electrocatalytic activity compared to Ni foam alone, evidencing its ability to contribute to efficient charge separation in the TiO2/SNGP/CdS-polysulfide/silica gel-PProDOT/CMS-BiNF cell.
(PProDOT)x+:(ClO4)x− (neutral) + y(ClO4−) ⇆ (PProDOT)(x+y)+:(ClO)(x+y)− (oxidized) + ye−. | (3) |
In case of carbon micro-spheres and Bi nanoflakes, they predominantly store and release charge by EDL formation and its collapse. The areal capacitance (ASC), energy density (E) and power density (P) for these electrodes in two electrode mode are determined using the following equation described below and these parameter values are provided in Table 2.
ASC (F cm−2) = (2 × I × Δt)/ΔV. | (4) |
E (W h cm−2) = 0.5 × ASC × ΔV2/3600. | (5) |
P (W cm−2) = 3600 × E/Δt. | (6) |
Current density, I (mA cm−2) | PProDOT//PProDOT | CMS-BiNF/PProDOT//PProDOT/CMS-BiNF | ||||
---|---|---|---|---|---|---|
ASC (mF cm−2) | E (μW h cm−2) | P (mW cm−2) | ASC (mF cm−2) | E (μW h cm−2) | P (mW cm−2) | |
0.05 | 117.7 | 16.3 | 0.05 | 180.8 | 25.1 | 0.05 |
0.07 | 97.6 | 13.5 | 0.07 | 130.3 | 18.1 | 0.07 |
0.1 | 56.7 | 7.8 | 0.1 | 89.0 | 12.4 | 0.1 |
0.3 | 51.8 | 7.2 | 0.3 | 69.0 | 9.6 | 0.3 |
0.5 | 48.2 | 6.7 | 0.5 | 57.0 | 7.9 | 0.5 |
0.7 | 47.6 | 6.6 | 0.7 | 53.2 | 7.3 | 0.7 |
1 | 47.0 | 6.5 | 1 | 50.0 | 6.9 | 1 |
In the above equations, I is current density in A cm−2, Δt is discharge time in s and ΔV is voltage window in V respectively. On decreasing the current density from 1 to 0.05 mA cm−2, the discharge time increases for both cells. The PProDOT/CMS-BiNF electrode exhibits an ASC and E of 180.8 mF cm−2 and 25.1 μW h cm−2 compared to the pure PProDOT electrode (ASC = 117.7 mF cm−2 and E = 16.3 μW h cm−2), which confirms that the charge storage capacity of the composite is enhanced in contrast to that of the pristine polymer, due to the availability of more number of electrochemically accessible active sites and lower charge transfer resistance, bestowed by the Bi nanoflakes and carbon micro-spheres. Carbon micro-spheres and Bi nanoflakes also serve as buffering layers for the polymer, PProDOT and prevent the swelling and shrinkage of the polymer during repetitive charge–discharge cycles. The role of Bi nanoflakes as a supercapacitor material is confirmed from CV and GCD plots over a voltage range from 0 to 1 V, given in Fig. S6 (ESI†). From the CV plot, a quasi-rectangular shape is observed in the scan rate range from 10 to 100 mV cm−2. The GCD plot shows an almost triangular shape and the ASC, E and P are determined to be 12 mF cm−2, 1.7 μW h cm−2 and 0.05 mW cm−2, by applying a current density of 0.05 mA cm−2.
There is no redox peak observed in the CV plots. Bi nanoflakes increase the electrical conductivity of the electrode, and improve the overall charge storage response by functioning as a material that can allow electrical double layer formation. However, the composite electrode of PProDOT/CMS-BiNF stores and liberates charge via pseudocapacitive and EDL capacitance mechanisms, because PProDOT is a redox polymer, and undergoes oxidation and reduction during the anodic and cathodic sweeps. These processes are kinetically fast, and therefore redox peaks are not observed at the said scan rates of 10–300 mV s−1 (Fig. 5a). However, in a CV plot for PProDOT recorded at a low scan rate of 2 mV s−1 (Fig. S7, ESI†), oxidation and reduction peaks are clearly observed at 0.45 V and 0.3 V respectively. The reversible doping and de-doping reactions are responsible for the observed peaks (eqn (3)). These peak positions agree well with that observed for a PProDOT derivative, in a tetrabutylammonium hexafluorophosphate electrolyte.52
On comparing performances with the literature studies on conducting polymer based supercapacitors, we found a study by Xiang et al. that reported a spherical composite having a yolk–shell structure of PProDOT and resin-based carbon spheres (PProDOT/YRFC) and the solid structure of the same (PProDOT/SRFC) having specific capacitances (SCs) of 327.5 and 180.9 F g−1 at a current density of 1 A g−1. PProDOT/YRFC showed a SC retention of 87.3% after 10000 charge/discharge cycles, owing to its uniformly dispersible fluffy structure.53 Kim et al., reported ternary silver/manganese oxide/polyaniline (Ag/MnO2/PANI) thin films which exhibited a SC of 800 F g−1 and a cycling stability of up to 83% compared to the pure PANI polymer (66%).54 A hierarchical N-doped porous carbon fiber@Cu (NPCF@Cu) composite based supercapacitor was reported by Hui et al., where a SC of 210 F g−1 was achieved by NPCF@Cu-10 higher than NPCF@Cu-0 (130 F g−1) and NPCF-10 (105 F g−1) at a discharge current density of 50 F g−1.55 Cu NPs increased the electrical conductivity of the composite, allowed rapid electron transport and lowered the charge transfer resistance, thus maximizing the SC. A similar role is possibly played by Bi nanoflakes here, for the composite with Bi (PProDOT/CMS-BiNF) has a higher electrical conductance than that of PProDOT/CMS or PProDOT. Our values of SC are comparable to the literature reports.
EIS studies provide insights on charge transfer and transport phenomena in the supercapacitors. Fig. 5e shows Nyquist plots for symmetric cells of PProDOT, PProDOT/CMS and PProDOT/CMS-BiNF electrodes over a frequency range of 0.1 Hz to 1 MHz which show a distorted semicircle over the high to intermediate frequency range followed by an inclined straight line in the low frequency region. The data are fitted into a circuit of [Rb(Q[RctW])Cdl]. Rb, Rct, Q, W and Cdl correspond to the bulk resistance of the electrolyte, charge transfer resistance at the electrode/electrolyte interface, constant phase element, Warburg diffusion coefficient and double layer capacitance respectively. Rct is the highest for the pure polymer cell, and comparable for the cells based on PProDOT/CMS and PProDOT/CMS-BiNF electrodes, indicating that carbon micro-spheres predominantly govern the interfacial resistance for charge transfer. The Warburg diffusion coefficient is the largest for PProDOT/CMS-BiNF (88.5 mΩ−1 cm2) compared to PProDOT/CMS (49.5 mΩ−1 cm2) and PProDOT (37 mΩ−1 cm2) (Table S6, ESI†). This large difference in the magnitudes confirms that ion diffusion is more efficient across the cross-section of the PProDOT/CMS-BiNF electrode, suggestive of carbon micro-spheres and Bi nanoflakes playing active roles in facilitating ion transport. They tend to occupy the spaces in between the polymer chains or coils, and thus separate out the chains, permitting ions to easily move through. Fig. 5f shows ASC (mF cm−2) and SC (F g−1) versus number of cycles for the PProDOT/CMS-BiNF electrode measured at a current density of 1 mA cm−2 corresponding to a gravimetric current density of 0.66 A g−1 over a voltage window of 0 to 1 V. In the first cycle, the electrode produces an ASC of 56 mF cm−2, while in the 5000th cycle it is characterized by an ASC of 47.6 mF cm−2. Thus, there is 85% retention of its initial ASC. Similarly, SC reduces from 36 F g−1 to 30.6 F g−1 from the 1st to the 5000th cycle. Thus, 82% of the initial SC is preserved after cycling. The loss in SC or ASC, is possibly due to active material loss with cycling.
Sn2− + 2e− → Sn−12− + S2−. | (7) |
S2− + 2h+ (CdS or SNGP) → S + CdS or SNGP. | (8) |
S + Sn−12− → Sn2− (n = 2–5). | (9) |
Scheme 3 Schematics of the PSC showing (a) charging under illumination and (b) discharging in the dark. |
These spontaneous reactions are evidenced from the photo-induced electrochemical parameters. Photovoltage versus time plots of PSCs based on symmetric supercapacitors based on the following electrodes: PProDOT, PProDOT/CMS and PProDOT/CMS-BiNF, are shown in Fig. 6a. In the first step, photo-charging was done, and no external voltage was applied. When illuminated by 1 sun (100 mW cm−2), the PSCs based on the said symmetric supercapacitors are charged to voltages in the range of 0.7 to 0.8 V within a second, and this voltage is sustained for 70 s. At this juncture, the illumination is switched off, the solar cell (A) is disconnected, and the PSCs are discharged under galvanostatic conditions. Under an applied fixed current density of 0.033 mA cm−2, the voltage across the PSC decays to zero volts for all the three supercapacitors. The discharge time is the longest for the ternary composite (PProDOT/CMS-BiNF) compared to PProDOT and PProDOT/CMS. Thus, the ASCs are calculated to be 104.6, 84 and 50.5 mF cm−2 for PProDOT/CMS-BiNF, PProDOT/CMS and PProDOT based PSCs respectively. The ASC, energy density (E) and power density (P) magnitudes are provided in Table 3. The higher ASC achieved by the PProDOT/CMS-BiNF electrode is attributed to the synergic interaction between the conducting polymer, carbon and metal nanoparticles, i.e., pseudocapacitive behavior of PProDOT, large effective surface area and electrical conductivity of carbon and Bi nanoflakes. Thus the internal resistance is reduced and ion and electron transport are facilitated. Bi nanoflakes also prevent the aggregation of the carbon microspheres and PProDOT chains, thus preventing charge trapping. Furthermore, repeated shrinking and swelling of the polymer via redox reactions also deteriorate cell performance; this is alleviated by the interspersed carbon-microspheres and Bi nanoflakes, which accommodate the localized volume change experienced by the polymer, thus imparting better cycling stability to the composite.
Supercapacitor | Discharge current density (mA cm−2) | Voltage (V) | ASC (mF cm−2) | E (μW h cm−2) | P (mW cm−2) |
---|---|---|---|---|---|
PProDOT | 0.033 | 0.72 | 50.5 | 3.6 | 0.024 |
PProDOT/CMS | 0.033 | 0.77 | 84.0 | 6.9 | 0.025 |
PProDOT/CMS-BiNF | 0.033 | 0.79 | 104.6 | 9.0 | 0.026 |
To examine the rate capability of the PSCs, the photovoltage decay plots were recorded for the PProDOT/CMS-BiNF electrode based PSC at different discharge current densities, and they are shown in Fig. 6b. When the discharge current density increases from 0.033 to 0.67 mA cm−2, the ASC varies from 104.6 to 27.1 mF cm−2. The highest energy density of 8.9 μW h cm−2 is obtained at the discharge current density of 0.033 mA cm−2 (Table 4). The PSC shows a good performance at low current densities. Self-discharge versus time plot for 70 s under 1 sun illumination is compared in Fig. 6c for the PSCs based on symmetric supercapacitors containing the PProDOT, PProDOT/CMS and PProDOT/CMS-BiNF electrodes. Both photo-charging and discharging (in the dark) of the PSC is performed without applying any voltage and discharge current. When the PSC is photo-charged for 70 s, a maximum voltage of 0.78 V is attained by the PProDOT/CMS-BiNF based cell. Once the light is switched off and solar cell is disconnected, there is an IR drop, the voltage drops to 0.7 V and gradually to 0.4 V at 500 s, and thereafter it remains constant. PSCs based on PProDOT/CMS and pure PProDOT show photovoltages of 0.74 V and 0.55 V, which decrease to 0.3 V and 0.17 V at 500 s. The IR drop is the least in case of the PProDOT/CMS-BiNF film, thus illustrating that this cell is superior to the other two cells.
Current density, I (mA cm−2) | ASC (mF cm−2) | E (μW h cm−2) | P (mW cm−2) |
---|---|---|---|
0.033 | 104.6 | 8.9 | 0.026 |
0.047 | 80.9 | 7.0 | 0.031 |
0.067 | 65.0 | 5.6 | 0.052 |
0.2 | 54.7 | 4.7 | 0.156 |
0.33 | 50.1 | 4.3 | 0.260 |
0.47 | 23.8 | 2.0 | 0.310 |
0.67 | 27.1 | 2.3 | 0.526 |
Photocurrent versus time curves for the PSCs are shown in Fig. 6d. During photo-charging for 70 s, a photocurrent maximum of 8 mA cm−2 is generated for the PProDOT/CMS-BiNF electrode. It is produced by the photo-excited electrons in the TiO2/SNGP/CdS photoanode of the solar cell, which are transmitted through the external circuit to the supercapacitor for charging, i.e., from (A) to (C) in the PSC (Scheme 3a).5 Thus, this current slowly decays to ∼6 mA cm−2 after 70 s and it roughly remains the same for the remaining duration of illumination. When light is switched off, under dark conditions and still under short-circuit conditions, (A) and (C) remain electrically connected, the photocurrent abruptly drops to negligible (close to zero) values, inferring that the current passing through the circuit is purely generated by photo-excitation. Similar profiles for current were also observed with the PProDOT/CMS and PProDOT electrodes, although the overall magnitudes of photocurrent maxima and saturation currents were lower than that achieved with the PProDOT/CMS-BiNF electrode. With these electrodes too, the photocurrent drops sharply to insignificantly small values, in the light switch off mode. These studies confirm that the TiO2/SNGP/CdS–S/S2−/SiO2 gel-PProDOT/CMS-BiNF@Ni foam connected to the CMS-BiNF/PProDOT//PProDOT/CMS-BiNF cell on a common current collector platform has tremendous potential as a dual function single device.
The overall photo-conversion and storage efficiency (ηoverall) of the PSC device is given by the following equation.
ηoverall = (EPSC × APSC)/(Elight × tch × AQDSC). | (10) |
In eqn (10), EPSC, Elight, tch, APSC, and AQDSC are the energy density of PSC, incident light power density (100 mW cm−2), photo-charging time, and the effective active surface areas of the supercapacitor part and the solar cell part of the PSC respectively. The energy storage efficiency of the PSC is given by the following equation.
ηstorage = ηoverall/ηconversion | (11) |
In eqn (11), ηstorage is the energy storage efficiency of the supercapacitor part in the PSC and ηconversion is the PCE of the solar cell in the PSC (9.41%). Thus, ηoverall and ηstorage of the PSC device are determined to be 6.8% and 72.3% respectively. Previously, Xu et al.,56 proposed a PEDOT-carbon supercapacitor integrated with the perovskite solar cell. The PSC reveals an ηoverall of 4.7% and an ηstorage of 73.77% respectively. Zhang et al.,57 reported an energy fiber PSC based on an integrating polymer solar cell with MWCNT sheets wrapped on a titania nanotube-modified Ti wire based supercapacitor. An ηoverall of 0.79% is obtained for this energy fiber device. A summary of ηconversion, ηoverall and ηstorage of PSCs is listed in Table S7 (ESI†). The cycling stability of the PSC can be gauged from Fig. 6e. The ASC versus time graph is plotted under light on/off conditions for 50 cycles. Photo-charging occurred for 5 s and galvanostatic discharging occurred after applying a discharge current density of 1 mA cm−2. The PSC gives a stable voltage over 50 cycles, indicating its stability and capability for storing charges repetitively.
Footnote |
† Electronic supplementary information (ESI) available: Figures for cyclic voltammograms of photoactive films, J–V plot of FTO/SNGP/CdS, Bode phase, LSV, CV and GCD plots of Bi nanoflakes, stability test of the solar cell. Tables of CB, VB data, five cell average, EIS data of photoanode and counter electrodes, literature survey for the overall efficiency of the PSC. See DOI: 10.1039/d0na00103a |
This journal is © The Royal Society of Chemistry 2020 |