Supattra Budsaereechaia,
Andrew J. Huntb and
Yuvarat Ngernyen*a
aDepartment of Chemical Engineering, Faculty of Engineering, Khon Kaen University, Khon Kaen, 40002, Thailand. E-mail: nyuvarat@kku.ac.th
bMaterials Chemistry Research Center, Department of Chemistry, Center of Excellence for Innovation in Chemistry, Faculty of Science, Khon Kaen University, Khon Kaen, 40002, Thailand
First published on 18th February 2019
Catalytic pyrolysis of waste plastics using low cost binder-free pelletized bentonite clay has been investigated to yield pyrolysis oils as drop-in replacements for commercial liquid fuels such as diesel and gasohol 91. Pyrolysis of four waste plastics, polystyrene, polypropylene, low density polyethylene and high density polyethylene, was achieved at a bench scale (1 kg per batch) to produce useful fuel products. Importantly, the addition of binder-free bentonite clay pellets successfully yielded liquid based fuels with increased calorific values and lower viscosity for all plastic wastes. This larger scale pyrolysis study demonstrated that use of a catalyst in powder form can lead to significant pressure drops in the catalyst column, thus slowing the process (more than 1 hour). Importantly, the use of catalyst pellets eliminated the pressure drop and reduced pyrolysis processing time to only 10 minutes for 1 kg of plastic waste. The pyrolysis oil composition from polystyrene consists of 95% aromatic hydrocarbons, while in contrast, those from polypropylene, low density polyethylene and high density polyethylene, were dominated by aliphatic hydrocarbons, as confirmed by GC-MS. FTIR analysis demonstrated that low density polyethylene and high density polyethylene oils had functional groups that were consistent with those of commercial diesel (96% similarity match). In contrast, pyrolysis-oils from polystyrene demonstrated chemical and physical properties similar to those of gasohol 91. In both cases no wax formation was observed when using the bentonite clay pellets as a catalyst in the pyrolysis process, which was attributed to the high acidity of the bentonite catalyst (low SiO2:Al2O3 ratio), thus making it more active in cracking waxes compared to the less acidic heterogeneous catalysts reported in the literature. Pyrolysis-oil from the catalytic treatment of polystyrene resulted in greater engine power, comparable engine temperature, and lower carbon monoxide (CO) and carbon dioxide (CO2) emissions, as compared to those of uncatalysed oils and commercial fuel in a gasoline engine. Pyrolysis-oils from all other polymers demonstrated comparable performance to diesel in engine power tests. The application of inexpensive and widely available bentonite clay in pyrolysis could significantly aid in repurposing plastic wastes.
Over the past two decades, a large number of results on catalytic pyrolysis process for plastic have been reported.4–14 A wide range of catalysts such as ZnO,4 MgO,4 CaCO3,5 CaC2,4 SiO2,4 Al2O3,4 SiO2–Al2O3,4 ZSM-5 zeolite,6–8 kaolin,9,10 red mud,8,11 CuCO3,12 and FCC,13,14 have been used. The present study attempts to utilise bentonite clay as an inexpensive and widely abundant material as a catalyst in the pyrolysis of waste plastic. Bentonite has been used in a limited number of studies for the pyrolysis of plastic including the pyrolysis of HDPE,15 PP,16 LLDPE16 and mixed plastic wastes.17 This initial proof of principle studies demonstrated that bentonite could be a suitable catalyst in pyrolysis process of plastics.16,18,19 Typically such catalysts have been utilised in a powder form which leads to a pressure drop that occur in catalyst column and further problems with the process.
The vast majority of these studies have only investigated the pyrolysis plastics on a lab scale (5–200 g).4,8,9,11,20–22 There are few literature examples that study pyrolysis systems on a larger scale. For example, Miandad et al. examine the effect of different plastic waste types, PS, PE, PP and PET, by using 1 kg of sample in pyrolysis reactor.23 Rehan et al. studied thermal and catalytic pyrolysis of 1 kg PS plastic waste by using a small pilot scale pyrolysis reactor.24 Such studies are key for understanding determining what parameters are important for scale up.
Herein, this work aims to investigate thermal and catalytic pyrolysis of plastic wastes, PS, PP, LDPE and HDPE, in bench scale reactor (maximum capacity 5 kg) using bentonite catalysts and compare the properties of resulting oils with commercial fuels, diesel and gasohol 91. This current study uses a bench scale reactor (1 kg per batch) and importantly the information gathered is transferable to a real production scale situation, and can be used for further scale up. Importantly, this current study demonstrates that the utilization of binder-free compressed catalyst pellets at scale can eliminate the pressure drop that can typically occur in catalyst columns. Liquid propane gas (LPG) is used has the fuel for heating the system instead of electricity thereby reducing the cost of products. The received oils were also test with real engines, diesel pump and gasoline brush cutters, which are amongst the most commonly used engines in daily life. Typically previous studies on the pyrolysis of plastics have focused on the characterization of their products; solid, liquid and gas, but few literature examples have tested the resulting liquid product with real engines. In the cases that engine studies have been undertaken only simulation engine have been used and have not been tested in actual machinery.10,25 It should be noted that this work uses gasohol 91 (not gasoline 95) to comparison with pyrolysis oil. This is due to the fact gasoline 95 is costly and not widespread throughout Thailand, as such gasohol 91 is representative of a fuel utilised throughout the region.
The thermogravimetric analysis of plastic waste samples was performed with a Shimadzu TGA-50. Typically 20 mg samples were placed in a 4 mm diameter platinum pan. The thermal decomposition experiments were carried out from room temperature to 700 °C at a heating rate of 10 °C min−1. The system was constantly purged with 10 ml min−1 of N2 to ensure pyrolysis conditions inside the TGA furnace. For each experiment, data of weight loss (%) and temperature (°C) were recorded.
The clay sample was characterized porosimetry by N2 adsorption–desorption isotherms at 77 K in ASAP 2020 Micromeritics equipment. Prior to the adsorption measurement, the sample was first degassed at 110 °C under vacuum until pressure <50 mmHg to remove moisture. Brunauer–Emmet–Teller (BET) method was used for surface area measurement. Total pore volume was evaluated from the adsorbed volume of nitrogen at P/P0 around 0.99. Micropore volume was calculated by the Dubinin–Radushkevich (DR) method. The average pore size was deduced using Barrett–Joyner–Halenda (BJH) method. The powdered clay was then compressed by hydraulic press at 50 bar to produce catalytic pellets with a diameter of 1 cm and length of 1.5 cm.
A bench scale fixed-bed pyrolysis stainless steel batch reactor (diameter 35 cm, length 60 cm, maximum capacity 5 kg) was used for production of oil from plastic packaging wastes (Fig. 1). 1 kg of plastic wastes was loaded into the reactor for each pyrolysis reaction. The reactor was heated externally by liquid propane gas to the required operating temperature at heating rates of 10, 15, 20 and 25 °C min−1. Reaction was carried out at 500 °C for 10 minute under a flow of nitrogen purge gas. The pyrolysis gas was passed through catalyst column at a ratio of 0.05, 0.1, 0.15 and 0.2 by weight of catalyst to plastic. The catalyst column made from glass (diameter 5 cm, length 100) and load with catalyst in pellet form. Pellets are formed on compression of the catalyst powder with hydraulic press at pressure of 50 bar, the resulting pellet have a diameter of 1 cm and length of 1.5 cm. No binder was used in the formation of the pellets. Fig. S1 in the ESI† demonstrates the bentonite clay, hydraulic press machine, palletization block and catalyst in pellet form. The resulting gas products were collected via water cooled condenser. The oil yield was determined based on the initial mass of plastic waste. A control experiment without catalyst was also conducted for comparison. It is important to note that the catalyst cannot be used in powder form when operating at a bench scale due to the generation of a significant pressure drop in catalyst column. As such typical literature examples that utilize catalysts in the powder form require long processing times (more than 1 hour) to pass the product gas through catalyst column and into the condenser to form the liquid product. By using the catalyst in a pellet form, the process time has been reduced to only 10 minute for pyrolysis of 1 kg plastic waste.
Fuel properties of the resulting pyrolysis oils were tested by the standard methods, including calorific value by bomb calorimeter, density by ASTM D1298, kinematic viscosity at 40 °C by ASTM D93, flash point by ASTM D93 and pour point by ASTM D79. The functional groups of oil were characterized by Fourier Transform Infrared spectroscopy (Bruker, Tensor 27) and the liquid fraction was analysed by Gas Chromatography Mass Spectrometry (PerkinElmer, TurboMatrix HS). The FTIR spectra of resulting oils were compare % similar with commercial fuels by using Bruker software.
The pyrolysis oils with and without using catalyst were used to operate both diesel and gasoline engines. A four-stroke engine, single piston diesel pump (HINOTA, ELP503) with maximum speed 3000 rpm, power 2.2 kW and maximum flow rate 40 m3 h−1 was used for diesel engine tests. A four-stroke engine gasoline brush cutter (Kanto, KT-NBC-4STK), with a 6000 rpm speed, power 2.6 kW and 40 cm3 displacement was used as a model petrol engine. The exhaust gas composition were analysed with an EMS 5002 gas analyser. Engine temperature was also measured by a GM700 infrared thermometer. The engine current was measured by a MX 655 multimeter and then converted to power.
The chemical composition of bentonite clay from product specification from Thai Nippon Chemical Industry Co., Ltd was found to be SiO2 46 wt%, Al2O3 17 wt%, Fe2O3 6 wt%, Na2O 1.5 wt%, CaO 2.5 wt% and TiO2 0.2 wt%. Bentonite clays have a similar composition to SiO2 and Al2O catalyst previously investigated as pyrolysis catalysts.6–8 Bentonite also had some compositional similarities to kaoline and red mud. The chemical compositions of kaoline were Al2O3 46.07 wt%, SiO2 43.12 wt%, TiO2 0.74 wt%, CaO 0.03 wt% and others while red mud had Fe2O3 36.5 wt%, Al2O3 23.8 wt%, TiO2 13.5 wt%, SiO2 8.5 wt%, CaO 5.3 wt%, Na2O 1.8 wt% and others.8,9 Low ratio of SiO2/Al2O3 indicated the acidity of the catalyst, thus highlighting the possible acidic nature of the bentonite catalyst.
Fig. 3 shows the N2 adsorption–desorption isotherms of the catalyst. According to the IUPAC classification, the shape of isotherm is type IV with the increasing in relative pressure, capillary condensation occurs. The hysteresis loop may be attributed to the mesoporous structure. Additionally, the steep jump observed at high relative pressure (>0.9) indicates some macropore existence.6 The BET surface area of bentonite clay was found to be 47 m2 g−1 with total pore volume 0.13 cm3 g−1. The micropore volume is 0.02 cm3 g−1 or 15% of total pore volume. The average pore size of the material was 10.9 nm and thus the catalyst was highly mesoporous.
Pyrolysis of plastic wastes without catalyst led to a brown coloured oil for PS and yellow for PP, LDPE and HDPE. Catalytic decomposition of the plastic waste had little effect on the colour of oil. Panda and Singh9 also found that the colour of oil obtained in catalytic pyrolysis of PP using silica, alumina and kaolin were yellow.
Table 1 indicates the comparison of oil yield with and without catalyst at different catalyst ratio. Presence of catalyst slightly increased the yield of oil as compare to without catalyst at all catalyst ratio. The use of a catalyst enhanced the ability to decompose or crack the polymer, thereby increasing the condensable gas yield and ultimately more liquid product.8 The advantages of the proposed pyrolysis system re that no char or wax is formed during the process. This is attributed to the acidic nature of the bentonite catalyst, which enabled the decomposition or cracking of waxes to lighter products. In contrast, Jan et al. used CaCO3 as catalyst for the pyrolysis of HDPE and found that wax formation occured.5 Mastral et al. also found that wax formed when undertaking pyrolysis of HDPE with HZSM-5 zeolite as an acidic catalyst.6 The highly acidic catalyst (low SiO2/Al2O3 ratio) was more active in cracking waxes compared to the less acidic catalyst (high SiO2/Al2O3 ratio).28 For bentonite clay, the ratio of SiO2:Al2O3 was 0.94, while HZSM-5 zeolite used in Mastral et al.6 had Si:Al ratio of 35. The wax is typically C13–C28 hydrocarbons and these components significantly decreased after using the bentonite catalyst, as shown in Table 2.
Catalyst:plastic ratio (by weight) | Oil yield (wt%) | Calorific value (kJ kg−1) | Density (g cm−3) | Viscosity (cP) | Flash point (°C) | Pour point (°C) |
---|---|---|---|---|---|---|
PS | ||||||
No catalyst | 86.4 | 43550 | 0.855 | 2.0 | 48 | 19 |
0.05 | 88.5 | 44547 | 0.843 | 1.8 | 51.2 | 17 |
0.10 | 87.9 | 44459 | 0.845 | |||
0.15 | 88.1 | 44696 | 0.839 | |||
0.20 | 88.2 | 44769 | 0.842 | |||
PP | ||||||
No catalyst | 89.5 | 43695 | 0.905 | 2.3 | 40 | 15 |
0.05 | 90.2 | 44659 | 0.906 | 2.0 | 44 | 15 |
0.10 | 90.5 | 44763 | 0.898 | |||
0.15 | 90.0 | 44776 | 0.902 | |||
0.20 | 89.9 | 44896 | 0.904 | |||
LDPE | ||||||
No catalyst | 85.6 | 43390 | 0.911 | 2.5 | 45 | 24 |
0.05 | 86.6 | 44121 | 0.905 | 2.0 | 57 | 21 |
0.10 | 87.0 | 44251 | 0.901 | |||
0.15 | 86.9 | 44395 | 0.904 | |||
0.20 | 87.6 | 44436 | 0.893 | |||
HDPE | ||||||
No catalyst | 86.9 | 43646 | 0.916 | 2.5 | 50 | 24 |
0.05 | 88.7 | 44191 | 0.910 | 2.0 | 59 | 24 |
0.10 | 88.4 | 44351 | 0.902 | |||
0.15 | 88.9 | 44661 | 0.905 | |||
0.20 | 88.7 | 44750 | 0.901 | |||
Diesel | ||||||
— | — | 46951 | 0.875 | 2.5 | 63 | 3 |
Gasohol 91 | ||||||
— | — | 45940 | 0.802 | 1.5 | 41 | — |
Component | %Area | |||
---|---|---|---|---|
No catalyst | Catalyst | |||
Aromatic | Non-aromatic | Aromatic | Non-aromatic | |
PS | ||||
C5–C9 | 60.22 | 0.44 | 61.80 | 1.74 |
C10–C13 | 1.00 | 0.00 | 1.00 | 0.43 |
C13 | 34.77 | 3.57 | 31.53 | 3.50 |
PP | ||||
C5–C9 | 6.26 | 18.65 | 10.94 | 21.45 |
C10–C13 | 2.20 | 7.76 | 1.44 | 15.05 |
C13 | 13.50 | 61.63 | 10.10 | 40.22 |
LDPE | ||||
C5–C9 | 3.45 | 8.49 | 3.59 | 14.05 |
C10–C13 | 0.00 | 19.31 | 0.00 | 22.28 |
C13 | 0.96 | 67.79 | 0.00 | 62.08 |
HDPE | ||||
C5–C9 | 2.52 | 13.79 | 3.12 | 14.72 |
C10–C13 | 0.00 | 21.18 | 0.00 | 21.43 |
C13 | 0.00 | 65.45 | 0.00 | 62.73 |
Diesel | ||||
Aromatic | Non-aromatic | |||
C5–C9 | 2.1800 | 1.1500 | ||
C10–C13 | 0.6300 | 11.1700 | ||
C13 | 0.5000 | 84.3700 | ||
Gasohol 91 | ||||
Aromatic | Non-aromatic | |||
C5–C9 | 43.2700 | 50.5200 | ||
C10–C13 | 1.0800 | 5.1300 | ||
C13 | 0.0000 | 0.0000 |
After apply catalyst a liquid yield more than 87% was obtained. López et al. used ZSM-5 and red mud as catalyst for the pyrolysis of mixed plastic wastes and found that the maximum liquid yield were 56.9 and 76.2 wt%, respectively.8 Shah et al. also found that liquid product yields were in the range 62–79% when using ZnO, MgO, CaC2, SiO2, Al2O3 and SiO2–Al2O3 as catalysts in pyrolysis of LDPE.4 The system in this current work can obtain high liquid product with small amount of catalyst (catalyst to plastic waste ratio of 0.05) and at short reaction times (10 min). For example, optimum conditions for pyrolysis of HDPE with CaCO3 are catalyst ratio of 0.2 and reaction time of 1.5 h.5 Panda and Singh also used catalyst ratio of 0.33 with reaction time of 75 min to received highest yield of liquid product around 89.5 wt% by pyrolysis of PP with kaoline.9 The catalyst ratio of 0.2–0.4 and pyrolysis time of 1–3 h were also used with ZnO, MgO, CaC2, SiO2, Al2O3 and SiO2–Al2O3 as catalysts for the pyrolysis of LDPE.4
The catalyst did increase calorific values of the pyrolysis-oil to levels that were comparable to commercial fuels, diesel and gasohol 91 – the mixture of 90% gasoline and 10% ethanol, which had value of 46951 and 45940 kJ kg−1, respectively. Literature values reported the calorific value of diesel to be between 43800–48610 kJ kg−1.10,21 These literature values are in good agreement with the results obtained in this work, which demonstrated calorific values of 44896 kJ kg−1 for PP with a catalyst:plastic ratio of 0.2 (by weight). The standard calorific value of commercial gasoline is reported as being 45600 kJ kg−1, this figure is identical to the calorific value for gasohol 91 used in this current study.4 The calorific value of oil obtained from pyrolysis of plastic in this work was comparable to other studies. Panda and Singh who used silica alumina and kaolin as catalysts for the pyrolysis of PP, found that the received oil had calorific value of 47120 and 47095 kJ kg−1, respectively.9 Shah et al. demonstrated that, after using ZnO, MgO, CaC2, SiO2, Al2O3 and SiO2–Al2O3 as pyrolysis catalysts for LDPE, the calorific value of oils were in the range 40500–45000 kJ kg−1.4 This value is comparable when using bentonite (44121–44436 kJ kg−1). Kumar et al. who used kaolin as a catalyst for the pyrolysis of HDPE, demonstrated that the resulting oil had a calorific value of 40170 kJ kg−1, that is lower than those obtained when using a bentonite clay, as demonstrated in this work (44191–44750 kJ kg−1).10 Therefore, high calorific value of the obtained oils in this study by using catalyst showed their potential as alternatives to commercial fuel.
Application of the bentonite catalyst had little significant effect on the density of pyrolysis oil did. The densities of oil from PP, LDPE and HDPE had higher than that of PS, which is close to density of diesel and gasohol 91. Abu-Hamdeh and Alnefaie indicated that the density of diesel was 0.848 g cm−3, and close to the values for pyrolysis oils reported in this current work (0.875 g cm−3).21 In contrast, to other studies that have reported pyrolysis oil densities from HDPE of up to 1.12 g cm−3,29 the results in this current study demonstrate promise for use in liquid fuel applications (0.898–0.906 g cm−3).
A viscosity of 1.8 cP was observed for pyrolysis-oil for PS when using catalyst, encouragingly this has a viscosity close to gasohol 91 (1.5 cP). The viscosity of PP, LDPE and HDPE were 2.0 cP and close to that of diesel (2.5 cP) (Table 1). The viscosity of commercial diesel as reported in literature is in the range of 2.0–4.5 cP.29 In contrast to the application of bentonite clays as catalysts in this work, Chen et al. investigated the viscosity of oil from pyrolysis HDPE and reported viscosities of 2.96 cP.29 Previous studies on the catalytic pyrolysis of PP with silica alumina and kaolin yielded pyrolysis oils with viscosities 2.21 and 2.27 cP, respectively.9 While Kumar et al. reported that oil from catalytic of kaolin of HDPE had viscosity of 2.1 cP.10 These results are comparable to those obtained in this current work using bentonite clay (2.0 cP).
The flash point of the pyrolysis-oil (liquid products) increased when processing in the presence of the clay catalyst. Pyrolysis-oils produced from LDPE and HDPE in the presence of the bentonite clay had flash points close to that of commercial diesel. In contrast, PS and PP pyrolysis-oils also produced with bentonite catalysts exhibited flash points close to gasohol 91. The standard values of flash point for diesel and gasoline are 55–60 and 37.8–38 °C,4 respectively, which in agreement with this research. Bentonite is therefore an effective catalyst for the production of a diesel alterative from waste LDPE and HDPE. Shah et al. reported the flash point of catalytic oils when using ZnO, MgO, CaC2, SiO2, Al2O3 and SiO2–Al2O3 catalysts in the range of 30–62 °C.4 Jan et al. demonstrated the use of CaCO3 in catalytic pyrolysis of HDPE and yielded an oil with a flash point of 50 °C.5
Comparison of the pour point of resulting oils and commercial fuels is presented in Table 1. The pour point of gasohol 91 was not measured in this work due to the high volatility of the sample. This consistent with other research that did not measure the pour point of gasoline.5 Jan et al. reported that there are no standard value of pour point for diesel and gasoline.5 The pyrolytic oils from plastic wastes had higher pour point than diesel. For all plastic wastes investigated the use of the bentonite catalyst did not significantly affect the pour point of resulting oil. However, for PS and LDPE a small decrease in the pour point values were observed on application of the bentonite clay catalysts. Pour point is known as the temperature at which the fluid stops to flow. Generally, the increase in viscosity may cause the fluid losses its flow characteristic. This is in agreement for PS and LDPE results.
Pyrolysis with no catalyst yields highly active pyrolysis-oils that can undergo polymerisation to form solid materials. Unlike pyrolysis in the absence of catalysts, the pyrolysis-oil products under catalytic conditions were low viscous liquids, indicating the enhanced breakdown and cracking of plastic wastes into low molecular weight liquid hydrocarbons. These results are supported by GC-MS data of the oils (Table 2), indicating greater proportions of lower molecular weight hydrocarbon fractions, C5–C9 (aliphatic and aromatic compounds) were produced using catalysts, while higher molecular weight hydrocarbon fractions, C13, decreased. In conclude, the increasing amount of catalyst did not effect to the yield and fuel properties. Therefore, it is unnecessary to use high loadings of catalyst, leading to an optimum catalyst to plastic waste ratio of 0.05.
The pyrolysis-oil (liquid products of pyrolysis) from plastic wastes were analysed by GC-MS (Table 2). The identified compounds were categorised according to the length of their carbon chain: C5–C9, C10–C13 and C13. Those molecules with a chain length of C5–C9 comparable to the composition of gasoline, while C13 are heavy oils. It was observed that catalytic and non-catalytic pyrolysis of PS mainly yielded aromatic hydrocarbons with carbon number C5–C9 around 60% and C13 around 30%. These compounds are similar to those present in gasohol 91 more than diesel. It has been reported that one of the mechanisms of formation of aromatics during pyrolysis is via Diels–Alder reactions and subsequent dehydrogenation to form aromatic rings and it is probably related to the specific composition of the sample pyrolyzed.22 However, in the case of polystyrene, this feedstock is highly aromatic and as such would be likely to also yield aromatic products during catalytic pyrolysis. For PP, LDPE and HDPE, the resulting oils are mostly aliphatic hydrocarbons (alkanes and alkenes) with carbon number more than C13. These results were consistent with FTIR results.
The five most abundant compounds present in the pyrolysis-oils are summarized in Table 3. The pyrolysis of PS yielded, styrene (20.12%), ethylbenzene (15.07%), benzene, 1,1′-(1,3-propanediyl)bis- (11.17%), α-methylstyrene (10.38%) and toluene (7.93%). On application of the catalyst during pyrolysis, the mainly compounds remained the same, however, in the respective ratio of these components differed. Pyrolysis of PP produced an oil containing 2,4-dimethyl-1-heptene (15.08%), 1-tricosene (14.98%), 3-octadecene, (E)- (7.78%), 1-pentadecene (7.76%) and 1-decene, 2,4-dimethyl- (4.33%). Some compounds such as 1-nonadecene (7.38%), 1-hexadecene (7.27%) and 3-eicosene, (E)- (7.11%) appear with the use of the bentonite catalyst. For LDPE and HDPE, it was shown that pyrolysis-oils with and without catalyst had compounds like to diesel.
PS | PP | LDPE | HDPE | Diesel | Gasohol 91 | ||||
---|---|---|---|---|---|---|---|---|---|
NC | C | NC | C | NC | C | NC | C | ||
a NC = no catalyst, C = catalyst. | |||||||||
Styrene (C8H8, 20.12%) | Styrene (C8H8, 24.49%) | 2,4-Dimethyl-1-heptene (C9H18, 15.08%) | 2,4-Dimethyl-1-heptene (C9H18, 15.71%) | Eicosane (C20H42, 3.14%) | Hexadecane (C16H34, 3.47%) | Octadecane (C18H38, 3.43%) | Nonadecane (C19H40, 3.39%) | Hexadecanoic acid (C16H32O2, 7.07%) | Toluene (C7H8, 13.28%) |
Ethylbenzene (C8H10, 15.07%) | α-Methylstyrene (C9H10, 12.28%) | 1-Tricosene (C23H46, 14.98%) | 1-Tricosene (C23H46, 7.87%) | Hexadecane (C16H34, 3.12%) | Nonadecane (C19H40, 3.45%) | Nonadecane (C19H40, 3.43%) | Octadecane (C18H38, 3.38%) | Heptadecane (C17H36, 6.04%) | Pentane, 2,3-dimethyl-(C7H16, 4.83%) |
Benzene, 1,1′-(1,3-propanediyl)bis- (C15H16, 11.17%) | Ethylbenzene (C8H10, 11.29%) | 3-Octadecene, (E)- (C18H36, 7.78%) | 1-Nonadecene (C19H38,7.38%) | Nonadecane (C19H40, 3.11%) | Pentadecane (C15H32, 3.43%) | Hexadecane (C16H34, 3.32%) | Eicosane (C20H42, 3.31%) | Pentadecane (C15H32, 5.79%) | Heptane, 4-ethyl- (C9H20, 4.44%) |
α-Methylstyrene (C9H10, 10.38%) | Benzene, 1,1′-(1,3-propanediyl)bis- (C15H16, 10.88%) | 1-Pentadecene (C15H30, 7.76%) | 1-Hexadecene (C16H32, 7.27%) | Heptadecane (C17H36, 3.06%) | Heptadecane (C17H36, 3.33%) | Eicosane (C20H42, 3.31%) | Hexadecane (C16H34, 3.21%) | 9-Octadecenoic acid, methyl ester, (E)-(C19H36O2, 5.58%) | Benzene, 1,3-dimethyl-(C8H10, 4.23%) |
Toluene (C7H8, 7.93%) | Toluene (C7H8, 7.56%) | 1-Decene, 2,4-dimethyl-(C12H24, 4.33%) | 3-Eicosene, (E)- (C20H40, 7.11%) | Pentadecane (C15H32, 2.98%) | Eicosane (C20H42, 3.25%) | Heptadecane (C17H36, 3.27%) | Heptadecane (C17H36, 3.19%) | Hexadecane (C16H34, 5.53%) | Octane, 2,3-dimethyl-(C10H22, 3.90%) |
All compounds identified in the resulting oils are presented in Table S1 of the ESI.† Although the major compounds did not demonstrate a significant difference in the oils products with and without a catalyst, significant differences can be observed in the minor compounds of the two oils. Some compounds including light hydrocarbons only appear after using catalyst, while heavy hydrocarbons disappear after using catalyst (Table S1 of ESI†). The oils obtained in the pyrolysis of plastic wastes under the optimum conditions of heating rate (10 °C min−1) and catalyst ratio (0.05 by weight) were characterised using FTIR (Table 4 and Fig. S1 of ESI†) provides the presence of different functional groups present in the oil. The FTIR spectra obtained for the pyrolysis oils with and without catalyst from PP, LDPE and HDPE are all similar, while PS significantly differs. The spectrum demonstrated d the presence of C–H stretches and consequently aromatic compounds between 3500 cm−1 and 3000 cm−1. PP, LDPE and HDPE also have dominate peaks which are between 3000 cm−1 and 2800 cm−1 showing the presence of –CH3, –CH2 and C–H groups. This illustrates the highly aliphatic nature of the oils products and consistence with GC-MS results. The peaks around 1600 cm−1 and 1494 cm−1 that occur only for PS and gasohol 91 represent CC stretching in aromatic ring. The peaks around at 1456 cm−1 and 1378 cm−1 relate to alkene and alkane structure, respectively. The absorption bands at 775 cm−1 and 695 cm−1 show the presence of aromatic compounds.
Wave number9,23,24 (cm−1) | Type of vibration9,23,24 | Nature of functional group9,23,24 | PS | PP | LDPE | HDPE | Gasohol 91 | Diesel | ||||
---|---|---|---|---|---|---|---|---|---|---|---|---|
NC | C | NC | C | NC | C | NC | C | |||||
a NC = no catalyst, C = catalyst. | ||||||||||||
3084, 3083 | C–H stretching | Aromatics | ✓ | ✓ | ||||||||
3078, 3075, 3060 | C–H stretching | Aromatics | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ||
3027, 3019 | C–H stretching | Aromatics | ✓ | ✓ | ✓ | |||||||
2956, 2954 | C–H stretching | Alkane | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | |||
2923, 2922 | C–H stretching | Alkane | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ||||
2872, 2871 | C–H stretching | Alkane | ✓ | ✓ | ✓ | ✓ | ✓ | |||||
1649, 1642, 1641 | CC stretching | Alkene/fingerprint region for phenyl ring substitution overtone | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ||||
1607, 1602 | C–C stretching in ring | Aromatics | ✓ | ✓ | ✓ | |||||||
1494 | C–C stretching in ring | Aromatics | ✓ | ✓ | ✓ | |||||||
1456, 1454, 1451 | CC stretching | Alkene/fingerprint region for phenyl ring substitution overtone | ✓ | ✓ | ✓ | ✓ | ✓ | |||||
1378, 1377, 1376 | C–H scissoring and bending | Alkane | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ |
909, 908, 906 | C–H bending | Alkene | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ||||
889, 888, 887, 877 | C–H out of plane bending | Alkene | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ||||
775, 774 | C–H “oop” | Aromatics | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ||||
729, 723, 722 | C–H rock | Alkane | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ||||
697, 696, 695 | C–H “oop” | Aromatics | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ | ✓ |
When compare FTIR spectra of oils with and without catalyst with commercial fuels, it can be observed that LDPE and HDPE are similar to diesel, with more than 96% similarity match, while PP similarity was more than 86%. For PS peaks, the using of catalyst increased % similarity with gasohol 91 from 63 to 66 (Table 5).
Type of plastic waste | % Similarity with diesel | % Similarity with gasohol 91 | ||
---|---|---|---|---|
No catalyst | Catalyst | No catalyst | Catalyst | |
PS | 17.90 | 20.75 | 63.20 | 66.35 |
PP | 86.18 | 87.63 | 58.67 | 61.01 |
LDPE | 96.89 | 96.08 | 56.78 | 62.80 |
HDPE | 96.75 | 96.53 | 56.95 | 62.75 |
Table 6 compares the pyrolysis conditions and % liquid yield between this work and literature published within 5 years. With the exception of Miandad et al.,35 the previously reported work on the pyrolysis of plastic was conducted on a small scale. The work conducted in this current study is one of the few examples of pyrolysis of plastic at a demonstrator scale. The pyrolysis temperature in this current work was consistent with previous studies, although the pyrolysis time was considerably shorter. This is due to the fact the pelletization of the catalyst eliminates any pressure drops that are typically associated with the use of catalysts in a powder form. Importantly, some of the literature indicated that waxes formation occurred when plastic pyrolysis took place in the absence of a catalyst. However in the current system, even in the absence of any catalyst limited wax formation was observed. This may be attributed to uniform controlled heating within the reactor and temperatures of 500 °C, which may lead to greater cracking of high molecular wax product into lighter hydrocarbons. Moreover, the bentonite clay is more acidic than other catalyst, therefore results in the cracking of waxes (C13–C28) into lighter hydrocarbon. Some catalyst used in literature such as CaCO3 and HZSM-5 lead to wax products. The yield of liquid product obtained from this work is comparable with those reported in the literature.
Researcher | Plastic | Pyrolysis conditions | Liquid yield (%) | |||||
---|---|---|---|---|---|---|---|---|
T (°C) | t (min) | Catalyst | Catalyst/plastic weight ratio | Reactor size (cm) | Scale | |||
a T = pyrolysis temperature; t = pyrolysis time; H = height of reactor, D = diameter of reactor. | ||||||||
This research | PS, PP, LDPE, HDPE | 500 | 10 | Bentonite clay | 0.05–0.2 | H = 60 | 1 kg | 85.6–89.5% for none catalyst |
D = 35 | 86.6–90.5% for using catalyst | |||||||
Anene et al.30 | PP, LDPE, PP + LDPE | 460 | — | CAT-2 zeolite | — | 200 mL | 10 g | 62–96% for none catalyst |
51–68% for using catalyst | ||||||||
Singh et al.31 | HDPE | 390 | 16 | CuCO3 | 0.02–0.09 | 2 L | 100 g | 85% for none catalyst |
90–94% for using catalyst | ||||||||
Ratnasari et al.32 | HDPE | 500 | — | MCM-41, ZSM-5 | 2 | H = 17.9 | 2 g | ∼80–83.15% for using catalyst |
MCM-41+ZSM-5 | D = 2 | |||||||
Kunwar et al.33 | HDPE | 400–475 | 180–360 | Y-zeolite | 0.1–0.2 | 2 L | 600 g | 86–93% for none catalyst |
MgCO3 | 29–84% for using catalyst | |||||||
Wax occur for none catalyst | ||||||||
Lerici et al.34 | PS, PP, LDPE, HDPE | 500 | 20 | H–Y zeolite | 0.5 | H = 30 | — | 42–71% for using catalyst |
D = 0.9 | Wax occur for none catalyst | |||||||
Miandad et al.35 | PS, PP, PE, PS + PP, PS + PE, PP + PE, PS + PE + PP, PS + PE + PP + PET | 450 | 75 | Natural zeolite | 0.1 | H = 36 | 1 kg | 14–60% |
D = 31 | ||||||||
Synthetic zeolite | 20 L | |||||||
Abdullah et al.36 | PS | 350–550 | — | None | — | H = 25 | 30 g | 7.11–84.8% |
D = 7.36 | Wax occur for all conditions |
The emission of carbon monoxide (CO) from engines fuelled by pyrolysis-oils and commercial fuels is shown in Fig. 5. Toxic CO emissions are primarily due to the lack of oxygen, poor air entrainment and incomplete combustion. It was found that pyrolysis-oils produced through the catalytic route led to a decrease in CO emissions as compared to commercial fuels. For diesel pump, the pyrolysis-oils from plastic wastes had CO emissions that were comparable to that of the commercial fuels for both engines. It should be noted that the maximum detection of CO and CO2 in the analysis system is 100% and importantly no fuels exceeded 0.1% emissions of CO. All experiments were repeat 3 times and results were found to be highly reproducible.
Fig. 5 CO and CO2 emission from (a) gasoline brush cutter and (b) diesel pump at speed of 2000 rpm (NC = no catalyst and C = catalyst). |
Fig. 5 also illustrates the carbon dioxide (CO2) emission for both engines. The results show that CO2 emissions from pyrolysis-oils of plastic wastes were higher than commercial fuels for both engines. However, the use of bentonite clay as a catalyst can significantly decrease the CO2 emission as compared to the uncatalysed product. It should be noted that both engines produced NOx in very low amounts and below the limits of detection for the system.
Fig. 6 shows the variation of the engine temperature with speed for gasoline brush cutter. At all speeds, the use of plastic pyrolytic oil slightly increases the engine temperature. However, the using of bentonite as catalyst was able to reduce the engine temperature significantly. The use of pyrolytic oil trended to increase engine power at low speed as shown in Fig. 6. Moreover, the application of the clay catalyst increases the engine power to greater than that of the commercial fuel for all speed.
The engine temperatures of the diesel pump when using non-catalysed and catalysed pyrolysis-oils of plastic wastes are shown in Fig. 7. It can be observed that the using oils from the pyrolysis of plastic wastes increase the engine temperature when compare with commercial fuel. Addition of bentonite catalyst in pyrolysis process can decrease the engine temperature for all type of plastic wastes. Fig. 7 also shows the comparison of the engine power from produced oils with diesel. It was found that waste plastic oils have comparable engine power to that of commercial diesel.
Fig. 7 (a) Engine temperature and (b) power of diesel pump at speed of 2000 rpm (NC = no catalyst and C = catalyst). |
Importantly, few studies have reported the use or testing of the resulting pyrolysis oil in real engine test such as motorbike. When engine tests are conducted, these are almost always carried out in simulation engine such as DI engine. This current tested the pyrolysis oil as a fuel for a diesel pump and a gasoline powered brush cutter. For widespread use and uptake end users must have confidence that performance of the pyrolysis oil fuel will be equal or better than the current gasoline/diesel on the market and should not adversely affect the lifetime of the machinery. Therefore further testing on real engines not only helps to increase consumer confidence but can also provide crucial data on the performance of the fuel. It is recommended that economic assessment of processes at a pilot scale will help promote the development of such technologies for fuel production. Significant research focusses on the use of electricity (electric furnaces) to carry out pyrolysis of the raw materials, while this current study uses LPG. The economic assessment and efficiency comparison of these two approached would aid in evaluating the best route for production at a commercial scale.
In all cases catalyst reuse should be considered. A significant different between this work and previous studies in literature is the fact that the catalyst column is separate from the pyrolysis reactor. Typically the catalyst is used within pyrolysis reactor, thus leading to changes in catalyst structure through continual direct heating at pyrolysis temperatures. By implementing a separate catalyst column it may be possible to extend the catalysts lifetime. Catalyst reuse was attempted, it was demonstrated, that the received oil had identical yields and properties to those oils synthesized with fresh catalyst. Further testing is needed to truly assess the lifetime of such catalysts in pyrolysis processes.
This study clearly demonstrates the potential for making liquid fuels from waste plastic resources. The development of such technologies should be included in the national policies of growing nations and those that currently do not possess the necessary infrastructure to collect, separate and recycle plastic waste. The large scale application of pyrolysis technologies could be a viable solution for dealing with the growing problem of plastic waste worldwide and in a cost effective manner. The utilization of waste products such as plastic for energy generation would also go some way towards also meeting the increasing need for liquid fuels. Such technologies are still reliant on having effective collection systems to supply a constant stream of plastic waste. Governments should therefore encourage specific collection schemes order to meet the needs of such facilities, in addition to developing these technologies at scale. On an international basis, pyrolysis of plastic waste should be considered as a viable option for dealing with the growing volumes of plastic waste. However, it is vital that we not only solve this short term problem of plastic wastes but also in the longer term we must move towards the development of sustainable biobased plastics and fuels as part of a circular economy.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c8ra10058f |
This journal is © The Royal Society of Chemistry 2019 |