M. Coşkun*a,
Ö. Polat*b,
F. M. Coşkuna,
Z. Durmuşc,
M. Çağlard and
A. Türüta
aFaculty of Engineering and Natural Sciences, Department of Engineering Physics, Istanbul Medeniyet University, 34700 Üskudar, Istanbul, Turkey. E-mail: mustafa.coskun@medeniyet.edu.tr
bFaculty of Engineering, Department of Industrial Engineering, Istanbul Kultur University, 34156 Bakirkoy, Istanbul, Turkey. E-mail: o.polat@iku.edu.tr
cBağlar Mah., Gunesli Konutlar, No: 38, D-24, 34212, Bagcilar, Istanbul, Turkey
dFaculty of Science, Department of Physics, Anadolu University, Eskisehir, 26470, Turkey
First published on 25th January 2018
We have prepared LaCrO3 (LCO) and 10% Ir doped LCO samples by the solid state reaction method and studied the electrical modulus and the other dielectric properties of the samples by means of the impedance spectroscopy in the −100 °C to 100 °C range, with steps of 20 °C. It has been clearly observed that the dielectric properties change due to Ir doping. The absolute dielectric constant value of Ir doped LCO has decreased and this reduction was attributed to decreasing Cr6+ ions which may play a vital role in space charge polarization and charge hopping. A plateau region appeared in the temperature-dependent real electrical modulus M′ versus f curves of the pure LCO sample while almost no plateau region is visible in the Ir doped LCO sample. The temperature-dependent imaginary modulus M′′ versus f curves has two peaks at each temperature; one of the peaks is at low frequency and the other at the high frequency region, which shifts through higher frequency region with increasing temperature. This originates from free charge accumulation at the interface with the increase of the temperature. Furthermore, it has been seen that the Ir doped LCO sample has higher impedance and resistance values than the undoped LCO sample at the same frequency and temperature. This phenomenon was attributed to doped Ir ions behaving like a donor in LCO because LCO is a p-type compound. Moreover, the activation energy values of 0.224 eV and 0.208 eV for LCO and of 0.161 eV and 0.265 eV for the Ir doped LCO have been obtained from the slopes of the ρdc vs. (kT)−1 curves, respectively. Also the activation energies were calculated from the slopes of the fmax vs. (kT)−1 curves and the obtained results from low frequency region were in good agreement with ρdc vs. (kT)−1 ones.
LCO is one of those perovskite oxides has been studied extensively in the literature. LCO is a p-type compound with wide optical band-gap (3.4 eV), high electrical conductivity, high resistive to corrosive, high physical and chemical stability in ambient and has orthorhombic crystalline structure. The electrical, dielectric, magnetic and optical properties of LCO can be changed by doping both A (La) and B (Cr) cation sites with transition metals that offer excellent possibility to researchers to large application areas.35–38 The doped transition metal type has significant impact on the LCO properties because it changes almost all LCO parameter including physical and chemical. Many doping studies have been conducted on the LCO with various transition metals including Sr,39 Co,40 Ni,41 V,41 Cu,41 Mn,42 Ca,43 Pd44 etc.
The aim of the present study is to investigate how transition element iridium, Ir, affects the electrical properties of LCO. It has been well documented that the ionic radius of the doped/foreign cations and their mixed-valences are found to be the key parameters governing the electrical and magnetic properties of the parent materials. Ionic radius of Ir varies depending upon oxidation states, for instance, the ionic radius of Ir3+ is 0.068 nm but the ionic radius of Ir5+ is 0.057 nm. Moreover, in the literature, it has been shown Ir may have +1 to +9 oxidation states.45,46 Therefore, we have been inspired from such features of Ir element to study the electrical properties of LCO compound when it is doped by Ir. As far as we are concerned electrical and dielectric properties of Ir doped LCO study has not been conducted in the literature, yet.
We have experimentally investigated the absolute dielectric constant |ε|, electrical modulus |M|, impedance |Z|, the resistivity ρ, real M′ and imaginary M′′ of electrical modulus by means of the impedance spectroscopy of LCO and Ir doped LCO perovskite samples. The samples have been prepared by the conventional solid state reaction technique. The dielectric parameters versus frequency measurements have been conducted from −100 °C to 100 °C range with steps of 20 °C. Moreover, the ρdc vs. (kT)−1 and fmax vs. (kT)−1 curves have also been plotted to obtain the activation energy values of both samples.
Pure and Ir doped LaCrO3 powders were pressed into 13 mm pellets at 10 tons pressure for 1 minute. After that, the pellets were gradually heated to 1150 °C for 4 h in air to sinter the targets. Novocontrol Broadband Dielectric/Impedance Spectrometer was employed for frequency depended electrical and dielectric property measurements. Temperature of the samples was gradually varied from −100 °C to 100 °C with 20 °C step.
Fig. 1 (a and b) SEM images with different magnification (c) EDX analysis results for the pure LaCrO3 powders, respectively. |
Fig. 2 (a and b) SEM images with different magnification (c) EDX analysis results for the 10% Ir doped LaCrO3 powders, respectively. |
XPS analysis was employed in order to investigate oxidation stage of Ir doped LCO powder and obtained results are presented in Fig. 3. As can be seen from Fig. 3(a) XPS analysis of Ir 4f was fitted into the two doublets (four peaks) due to the oxidized and metallic forms of Ir. The peaks at 61.58 eV and 64.55 eV are corresponding the metallic Ir47 whereas the peaks at 62.95 eV and 64.55 eV are due to the oxidized form of Ir (4+),47 respectively. Therefore, it can be said Ir has mixed oxidation states of 0 and 4+ in the doped LCO. The ratio of peak areas for 0 and 4+ valance states also calculated via Gaussian fitting, which are 28.1% for O oxidation and 71.9% for 4+ valance states. Oxidation of Cr atom in LCO and Ir doped LCO has been studied as well. The peak levels at 575.61 eV and 577.10 eV showed that Cr has mixed oxidation sates of 3+ and 6+ (2p3/2)48 in our studied Ir doped LCO sample and data are given in Fig. 3(b). The Gaussian fitting reveals the ratio of peak areas of Cr3+ as 61.34% and Cr6+ as 38.66% in the investigated sample. Also the peak levels at 575.78 eV and 577.30 eV showed that Cr has both 3+ and 6+ oxidation states for undoped LCO too and the result was given at Fig. 3(e) and the Gaussian fitting reveals that the ratio of peak areas of Cr3+ as 56.8% and Cr6+ as 43.2%. Moreover, valence state of La has been inspected. Two peaks at 833.83 eV (for 3d5/2) and 850.60 eV (for 3d3/2) reveal the valance state of La is 3+ in Ir doped LCO sample.49 Finally, we have performed XPS analysis on the oxygen oxidation state. O 1s spectra have been investigated for Ir doped LCO sample. The obtained data have been represented in Fig. 3(d). It can be seen that O 1s spectra have high energy tail (second peak around 532 eV). Such tail of O 1s spectra are often seen in oxides and perovskite-like compounds. Even though the origin of these peaks is subjected to a number of discussions,50–55 Begreuther et al. introduced new ideas to illuminate the O 1s high energy tails.53 They expressed that the tails may be related to (i) the various oxygen states which belong to different chemical bonds between oxygen–metal atoms, (ii) the defects within the crystal structure. In our studied Ir doped sample the presence of various oxidation states of Ir (metallic and 4+) and/or defects support Begreuther et al. ideas. Both EDX and XPS inspections have demonstrated that the transition element Ir has been doped into LaCrO3 structure and also any impurity has not been observed in the these analysis results. Further, any extra peak has not observed in XRD results that confirm our compounds do not have impurity.44
Fig. 3 XPS analysis of (a) Ir 4f spectrum, (b) Cr 2p spectrum, (c) La 3d spectrum, (d) O 1s spectrum for Ir doped LCO and (e) Cr 2p spectrum for LCO. |
Fig. 4(a) and (b) represent the frequency (f) dependence of the dielectric constant |ε| in the temperature range from −100 °C to 100 °C with steps of 20 °C, (a) the pure LaCrO3 and (b) LaCr0.90Ir0.10O3, where |ε| is in terms of a magnitude (absolute value) of ε and the inset figures show temperature dependent dielectric constant |ε| with different frequency. As seen from Fig. 4(a) and (b), the dielectric constant increases with increasing temperature at a given frequency (see inset figures). At the frequency of 1.0 Hz, LCO sample has the ε values of approximately 104 at −100 °C and 3 × 107 at 100 °C, whereas 10% Ir doped LCO sample has the |ε| values of approximately 180 at −100 °C and 6 × 105 at 100 °C. That is, LCO sample has higher ε value than the Ir doped LCO sample at a given frequency. We believe that such decrease in |ε| value might be related to reduction of the number of Cr6+ ions, which may play a vital role on space charge polarization and charge hoppings, in LCO parent material due to substitution of Ir4+ ions. Liu et al. have shown that Sr doping into La in LCO structure boosts the conductivity and dielectric constant due to the generation of more Cr6+ ions.56 The XPS analysis confirmed that even though Cr3+ concentration increases from 56.8% to 61.34% for LCO and Ir doped LCO, the Cr6+ concentration lowers from 43.2% to 38.66% (see Fig. 3). Furthermore, it has been observed the plateau in the dielectric constant vs. frequency curves of LCO sample at each temperature. For example, the plateau of the curve for LCO at −100 °C ranges from approximately |ε| = 180 at 102 Hz to |ε| = 125 at 104 Hz, and plateau of the curve at 100 °C begins from |ε| = 240 at 3 × 105 Hz and beyond 107 Hz. The frequency range of the plateau in the |ε|–f curves of LCO sample increases with increasing temperature again, the dielectric constant of LCO sample sharply decreases with increasing frequency to the starting point of the plateau at each temperature. Moreover, it can be seen from Fig. 4(a) and (b), the plateau for the doped LCO sample becomes more pronounced with increasing temperature while the plateau for the pure LCO sample has been observed at each temperature. The dielectric constant of LCO and Ir doped LCO samples sharply decreases with increasing frequency to a given frequency and then more slightly decreases to further frequencies at each temperature. The low and high frequency plateaus are attributed to extrinsic contributions from grain and grain boundary effects, respectively.
Fig. 5 shows the frequency dependence of the electrical modulus of (a) LCO and (b) Ir doped LCO samples, in the temperature range from −100 °C to 100 °C, where |M| is in terms of a magnitude (absolute value) of the electrical modulus M also the inset figures show electrical modulus vs. temperature with various frequencies, 102, 103, 105 and 107 Hz. The electric modulus physically corresponds to the relaxation of the electric field in the material, so that the electric modulus represents the real dielectric relaxation process. The complex electric modulus, M* = M′ + jM′′, is inversely proportional to permittivity of the material, M* = 1/ε*. The Complex modulus also provides an alternative approach (i) to analyze the electrical response of the materials and has been adopted by scientists to study relaxation phenomena in ceramics materials and ionic conductors,17–24 (ii) helps to confirm the ambiguity arising from the grain or grain boundary effect at elevated temperatures which may not be distinguished from complex impedance plots. The complex electric modulus has been discussed with both permittivity and impedance to study and analyze the contribution of the grain boundary on the relaxation mechanism of the materials also it offers us opportunities to investigate long-range conductions and localized dielectric relaxation phenomenon in microscopic level.17–24 The complex electric modulus is the inverse of complex permittivity and is given as follows:17
(1) |
Moreover, it can also be expressed in terms of a derivative of complex impedance Z*.17
M* = M′ + jM′′ = jwε0Z* = jwε0Z′ − wε0Z′′ | (2) |
Fig. 6 shows the frequency dependence curves of the real part of electrical modulus, M′, in the temperature range from −100 °C to 100 °C, (a) parent material LCO, inset shows the log–log plots of the real part of modulus with frequency; (b) shows temperature dependent real part of electrical modulus with different frequency of LCO, (c and d) display the log–log plots and semi-log of the real part of modulus of the Ir doped LCO as function of applied frequency and inset figure (c) shows temperature dependent real part of electrical modulus Ir doped LCO, respectively. When looking at the temperature-dependent M′ versus f curves of both samples, the M′ value increases with decreasing temperature at each frequency (see inset figures (b) and (c)), and it clearly seems that there is a difference in graphics due to the doped Ir. For example, in the log–log plots, the M′ versus f curve of LCO sample ranges from approximately 1.6 × 10−6 at 1.0 Hz to 6 × 10−2 at 107 Hz for −100 °C, however, the curve of the Ir doped LCO varies from approximately 3 × 10−3 at 1.0 Hz to 7 × 10−2 at 107 Hz for −100 °C. When we look at the applied temperature of 100 °C, the curve of LCO ranges from around 8 × 10−11 at 1.0 Hz to 6 × 10−3 at 107 Hz, but the curve of the Ir doped LCO ranges from nearly 2.5 × 10−10 at 1.0 Hz to 4 × 10−2 at 107 Hz. That is, the M′ versus f curve of the Ir doped LCO sample changes in a narrower range compared to that of the pure LCO at −100 °C. The change range expands with increasing temperature. As can be seen from the Fig. 6, the real part of electrical modulus, M′, of both samples increases with boosting frequency at a given temperature, and it reaches a constant value at high frequencies. Moreover, when we look at the temperature-dependent semi-log M′ versus f curves of both samples, Fig. 6(a) inset and (c), a plateau region seems in the M′ versus f curves of LCO sample whereas no plateau region almost is visible in those of the Ir doped LCO sample at each temperature.
Fig. 7 shows the frequency dependence curves of the imaginary part of electrical modulus, M′′ in the temperature range from −100 °C to 100 °C with steps of 20 °C, (a) LCO and (b) the Ir doped LCO, respectively. It is clearly seen that step like behavior was observed for both parent LCO and Ir doped LCO. It is clearly realized from Fig. 7(a) and (b) that M′′ versus f curves have two peaks at each temperatures, one of the peaks is at low frequency and other at high frequency region. It can be noticed that those peaks moves to higher frequency region via escalation of applied temperature. Such shift originates from free charge accumulation at the interface with the increase of the temperature. Thus, the increase in the charge carrier mobility decreases the relaxation time. The fact that the peaks shift to the higher frequency region with the increasing temperature indicates that dielectric relaxation is a thermally activated process in which the hopping mechanism of charge carriers dominates intrinsically. As can be seen from the figures, both peaks of the Ir doped LCO sample appears in the studied frequency range, 1.0 to 10 MHz. The second peak for parent LCO sample shifts towards frequencies over 107 Hz at temperatures above −60 °C which is out of measurement frequency of our device. These peaks at low and high frequency regions demonstrate us that the mobility of ion migration from short time constant to long time constant passes via reducing frequency. The peak height in the M′′ versus frequency curves is proportional to capacitance, C−1, i.e. M′′max = C0/2C and here C0 is the empty capacitance of sample.
Fig. 7 Frequency dependence plots of the imaginary part of electrical modulus, M′′ in the temperature range from −100 °C to 100 °C with steps of 20 °C, (a) pure LaCrO3 and (b) LaCr0.90Ir0.10O3. |
Fig. 8 represents the frequency dependent-electrical modulus plane plots of both samples, the imaginary M′′ versus real M′ curves in the temperature range from −100 °C to 100 °C, (a) the parent LCO, inset: low frequency data of the complex electric modulus plane plot of LCO, and (b) the Ir doped LCO. The intercept on the real axis gives the capacitance from the grain or grain boundary. The semicircular arcs have been observed in the modulus plane plot of both samples in low and high frequencies, which points the presence of two relaxation processes. The small semicircular arcs at low frequency correspond to the contribution of weak grain boundary effects rather than the dominant grain effects. The large semicircular arcs at high frequency represent the bulk or grain response.17–24,31 A deviation from the semicircular shape of modulus arc of both samples has been observed with increasing temperature in high frequency region, and the semicircular arc for LCO sample has only formed at −100 and −80 °C, though the semicircular arc for the Ir doped LCO sample has only formed at the other frequencies except 60, 80 and 100 °C.
The activation energy Ea of the LCO and Ir doped LCO samples have been calculated by using M′′ vs. frequency plots. The M′′ vs. frequency plots for LCO and Ir doped LCO have two peaks, as can be seen from the Fig. 7. In order to calculate activation energies an Arrhenius formula used that is given in eqn (3).
(3) |
Fig. 9 fmax versus (kT)−1 plots of both LCO and Ir doped LCO samples. The solid lines represents the fits to the experimental data. |
Material | fmax (Hz) (at low f) | fmax (Hz) (at high f) | ||||
---|---|---|---|---|---|---|
f0 (Hz) | Ea (eV) | f0 (Hz) | Ea (eV) | |||
I | II | Ea1 | Ea2 | |||
LCO | 2.28 × 108 | 5.96 × 107 | 0.229 | 0.184 | 4.44 × 1011 | 0.196 |
Ir doped LCO | 1.52 × 106 | 9.58 × 107 | 0.211 | 0.307 | 5.22 × 109 | 0.223 |
The calculated activation energy values show that the hopping charged particles over the potential barrier are the origin of conduction mechanism for our compounds.62 Fig. 10 shows the Z′′ and M′′ vs. frequency plots at −100 °C and 100 °C for LCO and Ir doped LCO compounds. It is noticed from these plots, the Z′′ has single peak whereas the M′′ has two peaks, one of them is at low frequency region other is at high frequency region. It can be seen from Fig. 10(a) the peak of Z′′ and M′′ (low frequency peak) vs. frequency occurs at same frequency at −100 °C for LCO that suggests a delocalized relaxation mechanism and having long-range mobility.63 On the other hand, this behavior has not been observed for LCO at 100 °C (Fig. 10(b)) also at −100 °C and 100 °C for Ir doped LCO (a slight mismatch can be clearly seen from Fig. 10(b–d)) which suggests localized relaxation mechanism of long-range interaction.63
Fig. 10 Z′′ and M′′ vs. frequency plots (a) −100 °C, (b) 100 °C for LCO and (c) −100 °C, (d) 100 °C for Ir doped LCO compounds. |
Relaxation time (τ) can be inferred using the formula ωmaxτ = (2πfmax)τ = 1 in each peaks in the M′′ vs. frequency plots. Fig. 11(a) and (b) show the M′′ vs. frequency behavior for LCO and Ir doped LCO just at −100 °C and the relaxation points (ωmaxτ = 1) can be clearly seen for each compounds. I seen from Fig. 11 (inset figures) equivalent circuit composed from a two parallels RC elements that are connected in series. The relaxation time can be defined in terms of resistance (R) and capacitance (C) which are originating from grain and grain boundary as shown below:
τ = RC | (4) |
τg = RgCg, τgb = RgbCgb | (5) |
(6) |
(7) |
Fig. 11 The M′′ vs. frequency behaviour for LCO and Ir doped LCO just at −100 °C and the relaxation points (ωmaxτ = 1). Inset figures show equivalent circuit for each compounds. |
The capacitance values are determined using the M′′ vs. frequency plots due to the relation between M′′ = C0/2C at the relaxation points (ωmaxτ = 1) mentioned before. The calculated capacitance values for grain (Cg) and grain boundary (Cgb) are listed in Table 2. Now, we can calculate the resistance values for grain (Rg) and grain boundary (Rgb) using the eqn (5). The calculated R values were represented with together the capacitance values of Cg and Cgb in Table 2. Temperature dependent C and R plots are given in Fig. 12(a) and (b). It can be clearly seen that Cgb increases with increasing temperature and reaches a maxima then slightly decreasing with increasing temperature, for LCO. The Cg for LCO has just 3 points due to lack of relaxation points of the M′′ vs. frequency plots and as can be seen from the Fig. 12 (a) the Cg is the temperature independent. From the same figure, Cgb shows same behavior with the LCO one for Ir doped LCO and Cg is temperature independent at low temperature regions while slightly increasing with raising temperature at higher temperature regions. The temperature dependent both Rg and Rgb for both compounds show similar behavior decreasing with increasing temperature, as it is observed from Fig. 12(b). Furthermore, it is seen from the same figure, the Rgb is much greater than the Rg for both compounds that grain boundaries behave like insulator while grains behave like semiconductor.64
T (K) | LCO | Ir doped LCO | ||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|
τgb (s) | τg (s) | Cgb (F) ×10−11 | Cg (F) ×10−12 | Rgb (Ω) | Rg (Ω) | τgb (s) | τg (s) | Cgb (F) ×10−11 | Cg (F) ×10−11 | Rgb (Ω) | Rg (Ω) | |
173 | 2.26 × 10−3 | 1.65 × 10−7 | 3.38 | 5.58 | 6.68 × 107 | 2.96 × 104 | 8.75 × 10−2 | 5.80 × 10−5 | 2.41 | 1.07 | 3.63 × 109 | 5.42 × 106 |
193 | 5.26 × 10−4 | 4.74 × 10−8 | 3.63 | 5.55 | 1.45 × 107 | 8.55 × 103 | 3.06 × 10−2 | 1.93 × 10−5 | 2.48 | 1.06 | 1.24 × 109 | 1.83 × 106 |
213 | 1.55 × 10−4 | 1.53 × 10−8 | 3.90 | 5.58 | 3.97 × 106 | 2.74 × 103 | 1.03 × 10−2 | 6.81 × 10−6 | 2.53 | 1.06 | 4.07 × 108 | 6.43 × 105 |
233 | 5.31 × 10−5 | 4.26 | 1.25 × 106 | 3.75 × 10−3 | 2.33 × 10−6 | 2.55 | 1.06 | 1.47 × 108 | 2.19 × 105 | |||
253 | 2.18 × 10−5 | 4.63 | 4.70 × 105 | 1.53 × 10−3 | 9.86 × 10−7 | 2.60 | 1.08 | 5.88 × 107 | 9.10 × 104 | |||
273 | 1.00 × 10−5 | 4.95 | 2.02 × 105 | 6.66 × 10−4 | 4.82 × 10−7 | 2.60 | 1.11 | 2.56 × 107 | 4.33 × 104 | |||
293 | 4.62 × 10−6 | 5.10 | 9.05 × 104 | 3.07 × 10−4 | 2.29 × 10−7 | 2.58 | 1.12 | 1.19 × 107 | 2.04 × 104 | |||
313 | 2.55 × 10−6 | 5.14 | 4.96 × 104 | 1.46 × 10−4 | 1.26 × 10−7 | 2.58 | 1.14 | 5.66 × 106 | 1.11 × 104 | |||
333 | 1.58 × 10−6 | 5.11 | 3.09 × 104 | 7.15 × 10−5 | 6.98 × 10−8 | 2.57 | 1.15 | 2.78 × 106 | 6.09 × 103 | |||
353 | 1.11 × 10−6 | 5.08 | 2.19 × 104 | 3.95 × 10−5 | 4.47 × 10−8 | 2.59 | 1.16 | 1.53 × 106 | 3.87 × 103 | |||
373 | 8.48 × 10−6 | 5.05 | 1.68 × 104 | 2.31 × 10−5 | 3.22 × 10−8 | 2.60 | 1.17 | 8.88 × 105 | 2.76 × 103 |
Fig. 12 Temperature dependent (a) capacity and (b) resistance plots of grain and grain boundary for LCO and Ir doped LCO. |
Fig. 13 shows the frequency-dependent plots of the impedance of both samples in the temperature range from −100 °C to 100 °C, (a) LCO sample and (b) the Ir doped LCO sample, where |Z| is in terms of a magnitude (absolute value) of the impedance Z. Generally, the total impedance acts as pure capacitance at higher frequencies and pure resistance at lower frequencies. Fig. 13(a) and (b) exhibit that the impedance value of both samples increases with decreasing temperature at a given frequency. LCO sample has the values of about 6.5 × 107 Ω at −100 °C and 3 × 104 Ω at 100 °C, and the Ir doped LCO sample has the values of about 3.5 × 109 Ω at −100 °C and 9.5 × 105 Ω at 100 °C at low frequency region. That is, the Ir doped LCO sample has higher impedance value than LCO sample at each temperature. Such higher impedance value of Ir doped LCO is most likely attributed to strain and distortion of in LCO crystal structure due to substitution of Ir with larger ionic radius into smaller Cr3+ ion. The presence of distortion probably causes the reduction of the pathway of the mobility charge carriers. As a result, the impedance increases and conduction decreases in the doped LCO sample. It is known that LCO is a p-type compound when Ir4+ substitutes Cr3+, a positive charge forms at Ir site and in order to maintain charge neutrality an electron will be created so Ir4+ behaves like a donor in the LCO. Consequently, every created electron causes decreases conductivity or increases impedance of Ir doped LCO.
Fig. 13 Frequency dependence of the impedance of both samples in the temperature range from −100 °C to 100 °C with steps of 20 °C, (a) pure LaCrO3 and (b) LaCr0.90Ir0.10O3. |
It is obvious from Fig. 13(a) and (b) the total impedance curves behave independent of frequency in low-frequency region and the frequency-dependent at high frequencies. The frequency range of the frequency-independent part of both samples decreases with increasing temperature. The frequency range of the frequency-independent part for LCO sample is wider than that of the Ir doped LCO sample at a given temperature.
Fig. 14 shows the frequency dependence curves of the phase angle in the temperature range from −100 °C to 100 °C, (a) LCO and (b) the Ir doped LCO samples. It can be realized from Fig. 14(a) and (b), both samples also have one peak each temperature. The peaks of the Ir doped LCO sample appear in the studied frequency range from −100 °C to 100 °C. Nevertheless, the peak of the pure LCO sample shifts towards frequencies over 107 Hz at temperatures above −40 °C, that is, out of our measurement frequency range. For both samples, the peak shifts towards high frequencies with increasing temperature. Another difference appears in the temperature-dependent phase versus frequency curves of both samples. As can be from the these figures, as phase angle, the zero degree starting point for the curves of the parent sample corresponds to 1.0 Hz at all temperatures; but, for the Ir doped sample it only corresponds to 1.0 Hz for the curves above −40 °C, and shifts to lower frequencies than 1.0 Hz with decreasing temperature at temperatures below −40 °C. Generally, the phase angle tends to be −90° at high frequency that the impedance is completely capacitive, and to 0° at low frequency that it becomes completely resistive, that is, the impedance approaches the R value at low frequencies.
Fig. 14 Frequency dependence of the phase angle of both samples in the temperature range from −100 °C to 100 °C with steps of 20 °C, (a) pure LaCrO3 and (b) LaCr0.90Ir0.10O3 samples. |
Fig. 15 illustrates the frequency dependence of the resistivity of both samples in the temperature range from −100 °C to 100 °C, (a) LCO sample and (b) the Ir sample doped LCO, respectively. It is well-known the total conductivity or resistivity of the sample composes of the frequency-independent dc bulk compound in low-frequency region and the frequency-dependent ac component. It is seen from Fig. 15(a) and (b) that the frequency range of the dc compound for LCO sample is wider than that of the Ir doped LCO sample at a given temperature. The resistivity decreases with increasing temperature at each frequency due to the increased mobility of oxygen vacancies or other structural defects.17–23,33,34
Fig. 15 Frequency dependence of the resistivity of both samples in the temperature range from −100 °C to 100 °C with steps of 20 °C, (a) pure LaCrO3 and (b) LaCr0.90Ir0.10O3. |
When Fig. 15(a) and (b) have been considered for the frequency-independent dc compound of the resistivity, ρdc, LCO sample has the values of around 1.6 × 108 Ω cm at −100 °C and 6 × 104 Ω cm at 100 °C, and the Ir doped LCO sample has the values of about 1.3 × 1010 Ω cm at −100 °C and 2.6 × 106 Ω cm at 100 °C. That is, the Ir doped LCO sample has higher ρdc value than LCO sample at each temperature. Jiang et al. have also found similar results when they introduced Ba2+ (ionic radius 0.161 nm) into La2+ (ionic radius 0.136 nm). They have demonstrated that the substitution of Ba2+ has generated distortion in the lattice, which caused scattering of the charge carriers and hence lowered the conductivity.65 We believe in Ir doped LCO sample we have similar situation because ionic radii of Ir4+ and Ir0 is larger than Cr3+ and Cr6+ ionic radii. So, there will be important distortion in the LCO lattice owing to Ir substitution. In the present study, the activation energy associated with the bulk conduction has been calculated from the intercept on the resistivity axis of the frequency-independent dc component at each measured temperature. The intercept values have been used for the ρdc versus (kT)−1 plot related to both samples in Fig. 16. The activation energy, cost must be paid by charge carriers to move inside the material, values of 0.224 eV at low temperature and 0.208 eV at high temperature for LCO, 0.161 eV at low temperature and 0.265 eV at high temperature for Ir doped LCO have been obtained from the slopes of the ρdc versus (kT)−1 curves, respectively. The obtained activation energy values are in good agreement with previous ones obtained from the slope of fmax vs. (kT)−1 curves.61 LCO has lower activation energy value at high temperature region than that at the low temperature region whereas the situation for Ir doped LCO is vice versa. The low activation energies show that hopping conduction is dominant mechanism for both samples. Materials with higher activation energy have higher resistivity than the materials with lower activation energy value. Therefore, our parent material LCO demonstrates less resistivity than the doped one.
Fig. 16 Resistivity versus (kT)−1 plots of both LCO and Ir doped LCO samples. The solid lines represent the fits to the experimental data. |
This journal is © The Royal Society of Chemistry 2018 |