Open Access Article
Sara
Gullace
a,
Matteo
Abruzzese
b,
Luca
Cusin
a,
Gabriele
Saleh
c,
Sanjay B.
Thorat
b,
Agnese
Gamberini
b,
Sebastiano
Bellani
b,
Artur
Ciesielski
a,
Francesco
Bonaccorso
bc and
Paolo
Samorì
*a
aInstitut de Science et d’Ingénierie Supramoléculaires, Université de Strasbourg, CNRS, 8 allée Gaspard Monge, 67000, Strasbourg, France. E-mail: samori@unistra.fr
bBeDimensional S.p.A., Via Lungotorrente Secca, 30R, 16163 Genova, Italy
cIstituto Italiano di Tecnologia, Via Morego, 30, 16163 Genova, Italy
First published on 17th August 2024
Lithium–sulphur batteries (LSBs) prevail as a viable alternative to Li-ion batteries due to their high theoretical specific capacity (1672 mA h gS−1). However, the formation of soluble polysulfides and their shuttle from the cathode to the anode cause irreversible capacity loss and uncontrolled self-discharge, limiting the performance of commercially available prototypes. In this work, we present a comparative analysis of two Kagome-shaped imine-based covalent organic frameworks (COFs) as functional modifiers for polypropylene (Celgard) separators in LSBs. We demonstrate, by using the KS60@Celgard separator modified with an optimized content of COF with the thienothiophene linker, the realization of LSBs reaching a specific discharge capacity of 850 mA h gS−1 at C5. The proposed separator has an extraordinarily high Li+ diffusion coefficient (DLi+) of 1.6 × 10−7 cm2 s−1 at the first cathodic peak, as well as the lowest S8
:
Li2Sx content ratio in the ex situ post mortem XPS analysis. These findings demonstrate that the use of separators modified with COFs allows the mitigation of shuttle effect, and is further accompanied by an efficient oxidation of Li2Sx to S8 (electrocatalytic effect). The equivalent K60@Celgard, based on a COF carrying a phenyl linker, results in LSBs with a specific discharge capacity of 599 mA h gS−1. This work highlights the synergistic effect of polysulfide retention, selective Li+ sieving and electrocatalytic activity of COF-modified Celgard separators in the development of high-performance LSBs.
A plethora of materials have been employed as functional separator modifiers, spanning from zero-dimensional (0D)20 to two-dimensional (2D) carbon-based materials,21 polymers,22 inorganic23 or hybrid polymer/inorganic materials.24–26 It has been demonstrated that the functional separator should provide a perfect balance between physical properties (i.e., surface area, pore volume and capillary forces) and electrochemical properties (Li+ transfer, C-rate capability and cycling stability). Such balance can be achieved using materials with ordered hierarchical pores.2,27
Based on this rationale, metal–organic frameworks (MOFs) and covalent organic frameworks (COFs) represent a viable attractive alternative as separator modifiers. In particular, COFs possess a highly ordered lattice structure and discrete hierarchical pores capable of interacting with ions and molecules.28,29 Furthermore, ad hoc chemical design enables the synthesis of COFs combining high surface area, low density, high stability to acids and bases, easy functionalization and ample combinations of building blocks, making them highly suitable for a wide range of applications, spanning from adsorption of contaminants and molecular sieving to catalysis, sensing, proton conduction and energy storage.30–33 In recent years, 2D COFs have been applied as sulphur-hosting materials in LSB cathodes, taking advantage of the highly ordered porous structure resulting from the stacking of the 2D planar sheets in one direction: this characteristic can provide accessible voids for sulphur impregnation, while suppressing the diffusion-driven loss of soluble polysulfides.34–36 However, the low electrical conductivity of this organic material composites represents an important weakness for the realization of practical electrodes.37,38 Nevertheless, COF-based materials offer structural designability to obtain abundant active sites for polysulfide adsorption, and accessible channels to facilitate the transport of Li+ and indirectly inhibit the growth of Li dendrites, enabling their use in advanced separators beyond their applications as electrode materials.39–42 Cao et al. reported the use of a sulfonate-rich COF-modified separator based on lithiated 3,5-triformylphloroglucinol and 2,5-diaminobenzenesulfonic acid (TpPa-SO3Li), obtaining a LSB with a specific discharge capacity of 939.4 mA h gS−1 at C5, along with 55.1% capacity retention after 100 galvanostatic charge/discharge (GCD) cycles, when using a cathode with a sulphur loading of 1.5 mgS cm−2.43 Similarly, Xu et al. used TpPa-(SO3)2 as a separator modifier, obtaining a specific discharge capacity of 879 mA h gS−1 at C10, in a LSB with a sulphur loading of 1.3–1.5 mgS cm−2 in the cathode. Additionally, they achieved a specific discharge capacity of 1036 mA h gS−1 at C5 with 82.5% capacity retention over 100 CGD cycles, when using a cathode with a sulphur loading of 3.2 mgS cm−2 and carbon nanotubes as advanced conductive additives44 (instead of the carbon black used in the low sulphur loading LSB and in ref. 43). Notably, these results were achieved using flat (carbon-coated) Al foils as current collectors, avoiding gas diffusion layers commonly reported for high sulphur-mass normalized performances, but leading to non-practical cell configurations (in terms of either gravimetric or volumetric full cell metrics).45,46
While hexagonal COF topology has received the greatest attention among LSB separators,43,44 in this work we present a comparative analysis of two Kagome-shaped imine-based COFs as functional modifiers for prototypical Celgard separators in LSBs. We discovered that COF KS1, carrying a thienothiophene linker, allows the corresponding LSB, encountering Celgard separators modified with a 60 wt% COF KS1-based coating, to achieve a specific discharge capacity of 850 mA h gS−1 at C5. Importantly, this cell was built with a cathode with a sulphur loading of 2.4 mgS cm−2 and a flat carbon-coated Al current collector. The proposed LSB exhibited a capacity retention of 74.1% after 190 GCD cycles. This result is accompanied by an extraordinary Li+ diffusion coefficient (DLi+) as high as 1.6 × 10−7 cm2 s−1 at the first cathodic peak. Under the same operating conditions, the use of a separator coating based on 60 wt% of COF K1, carrying a phenyl linker, results in LSBs with a specific discharge capacity of 599 mA h gS−1. Under the same operating conditions, also the increase of COF KS1 content in the separator coating (i.e., 80 wt%) results in a LSB with a poor specific discharge capacity of 577 mA h gS−1. The influence of the nature of the linker and the COF content on the performance of COF-modified Celgard separators for LSBs is also confirmed by post mortem ex situ X-ray photoelectron spectroscopy (XPS) and scanning electron microscopy (SEM) analysis. Our approach provides a strategy to cooperatively exploit the polysulfide retention, the selective Li+ sieving and the electrocatalytic activity of layered porous materials for the fabrication of high-energy density LSBs.
:
30 under magnetic stirring at 125 °C for ∼1 h, until complete sulphur melting and homogenization. The resulting composite was subsequently cooled down to room temperature and ground in a mortar. The S–SP composite was mixed through an appropriate mixer with SP and PVDF binder homogeneously dispersed in NMP, to obtain a slurry with 80
:
10
:
10 w/w ratio. The LSB cathodes were then obtained through casting of the prepared slurry on carbon-coated Al foil by means of a doctor blade with a height of 250 μm. The sample was subsequently dried at 50 °C for 3 h. Finally, the electrodes were cut into 14 mm-diameter disks (geometrical area of 1.54 cm2) and dried overnight under vacuum at 35 °C to remove traces of water and solvents.
:
DME 1
:
1 w/w mixture. An electrolyte to sulphur (E/S) ratio of 15 μL mgS−1 was used to fill the coin cells.
056 nm) at 40 kV and 40 mA and a LynxEye_2 detector (1D mode). Two Soller slits (Cu, 2.5 mm) have been applied to the primary and secondary optics. In the latter, a Ni stopper has been added to filter Cu kα radiation. XRD data were collected from 2 to 30° (2θ) with a step of 0.02° and an acquisition time of 1 s per step. Fourier transform-infrared (FTIR) spectra were acquired with a Thermo Scientific Nicolet iS50 FT-IR spectrometer equipped with the ATR diamond and a DTGS KBr detector. Thermogravimetric analysis (TGA) decomposition curves were recorded using a Mettler Toledo TGA/SDTA851e system in the range of 25–800 °C under a nitrogen atmosphere and with a heating rate of 10 °C min−1. X-ray photoelectron spectroscopy (XPS) characterization was performed using a Thermo Scientific K-alpha X-ray photoelectron spectrometer, equipped with an aluminum X-ray source (energy 1.4866 keV) at a vacuum level of 10−8/10−9 mbar in the analysis chamber. The spot size of the X-ray beam was fixed at 200 μm. Cyclic voltammetry (CV) measurements were performed with 0.1 mV s−1 scan rate in a potential window of 1.8–2.8 V vs. Li+/Li on a Biologic BCS-805 battery tester, while electrochemical impedance spectroscopy (EIS) measurements were performed in a frequency range of 500 kHz to 0.1 Hz with an amplitude of 10 mV using a VMP3B Multichannel Potentiostat. Galvanostatic charge–discharge measurements were performed at C5 (1C = 1672 mA gS−1) in a 1.9–2.8 V vs. Li+/Li potential window using a MACCOR series 4000 battery cycler. The C-rate convention (nC) is used in this manuscript, with 1C being defined as full theoretical lithium discharge/charge in one hour and n as the time (h) for complete charge or discharge at the nominal (theoretical) capacity.
The FTIR analyses of K1 and KS1 exhibit the typical spectral features of an imine-linked COF (Fig. S1c†), with bands ascribed to the imine C
N stretching vibration at 1616 cm−1 for K1 and at 1606 cm−1 for KS1.47 Moreover, the C
O stretching vibration bands (1683 cm−1 for TPA and 1653 cm−1 for TTDA) and the N–H vibration bands (3470–3320 cm−1 and 1620 cm−1) appear with significantly reduced intensities in the COFs, compared to the starting monomers. The most prominent bands at 1494 cm−1 for K1 and 1479–1497 cm−1 for KS1 are ascribed to the aromatic ring stretching modes.48
The PXRD analysis of TPDA–TPA and TPDA–TTDA provided evidence for a good degree of crystallinity of the two materials (Fig. S1d†). For COF K1, the main reflections at 2.5°, 4.2°, 4.9°, 6.4°, 8.7°, and 21.8° are ascribed to the (100), (110), (200), (210), (310), and (001) planes, respectively. In the case of COF KS1, the same pattern, slightly downshifted, was found at 2.3°, 3.9°, 4.6°, 6.0°, 8.2° and 21.1°, respectively. These PXRD patterns are in line with previous studies, which assigned to both COFs a Kagome structure with eclipsed stacking of the polymeric layers.47,49,50 However, our preliminary density functional theory simulations show unequivocally that the eclipsed structure is energetically unfavourable compared to other types of stacking (ESI Note 1†). The complexity of the reaction mechanism for the synthesis of COFs with the interplay between thermodynamic and kinetic effects,51 and, consequentially, their structural complexity would require a more accurate interpretation of the experimental PXRD patterns and those of the simulated structures to determine reliably the stacking geometry of these COFs (see also Fig. S13† and related discussion). However, this study goes beyond the scope of the present work.
TGA was performed to shed light onto the thermal stability of KS1 COF in a N2 atmosphere, while the analogous characterization of COF K1 has been already reported in our previous work.32 Fig. S1e† shows that KS1 is extremely robust and stable, with an initial 3 wt% loss in the temperature range between 110 °C and 170 °C, associated with the loss of physisorbed species, followed by its decomposition occurring after 430 °C.
COFs K1 and KS1 were characterized by XPS (Fig. S2 in the ESI†). The COF K1 high-resolution spectrum for C 1s core levels presents five deconvoluted sub-peaks at 284.4, 285.5, 286.3, 287.4 and 290.9 eV, which can be ascribed to the typical C
C, C–C, C–N, C
N chemical environments in the imine COFs, and the π–π* satellite for aromatic carbons, respectively. The N 1s spectrum confirms the presence of the triphenylamine moiety and the imine linkage, in addition to a small band for protonated amine, peaking at 398.4, 399.4 and 401.2 eV, respectively (Fig. S2a and b†). Similarly, the XPS spectra for COF KS1 can be deconvoluted to the same components, with the addition of a contribution from C–S at 287 eV in the C 1s core level (Fig. S2d†), as well as the S 2s and S 2p peaks (228.8 and 164.8 eV) in the survey spectrum (Fig. S2g†). In particular, the S 2p high-resolution spectra show the typical 2p3/2 and 2p1/2 doublets with an energy gap of 1.18 eV (Fig. S2f†).
:
Super P carbon black (SP)
:
polyvinylidene fluoride (PVDF), onto a prototypical battery separator, i.e., Celgard 2400 (Scheme 1b). In particular, separators coated with thin films with 60 wt% K1 and KS1 were named K60@Celgard and KS60@Celgard, while the separator coated with a layer based on a higher content of KS1, i.e. 80 wt%, is hereafter referred to as KS80@Celgard. Fig. 1a–c and S3† show the XPS spectra of the investigated COF-modified separators, i.e., K60@Celgard, KS60@Celgard and KS80@Celgard. The analysis reveals that the COFs K1 and KS1 maintain their structure in the composite coatings, while the appearance of a peak for F 1s in the survey spectrum is ascribed to the PVDF binder. SEM characterization shows that the COF K1 and KS1 morphologies are maintained, while sub-micrometric SP particles electrically connect COFs to each other (Fig. 1d–f). Fig. S4 in the ESI† shows the low-magnification SEM images of the pristine Celgard and COF-modified Celgard separators, as well as the SEM cross-sectional view of the pristine Celgard and the KS60@Celgard separator, evidencing the uniformity of the modified layers and thickness of the separator modifier, respectively (∼20 μm).
![]() | ||
| Fig. 1 (a)–(c) Survey XPS spectra for (a) KS60@Celgard, (b) K60@Celgard and (c) KS80@Celgard separators. (d)–(f) SEM images of the (d) KS60@Celgard, (e) K60@Celgard and (f) KS80@Celgard separators. | ||
Additionally, the Li+ diffusion coefficient (DLi+, expressed in cm2 mol−1) can be evaluated from the relationship between the peak current intensity Ip and the square root of the potential scan rate ν, as described by the Randles–Sevcik equation:
485 C mol−1), A is the electrode geometric area (1.54 cm2), C stands for the estimated Li+ concentration in the electrode volume expressed in mol cm−3, ν is the scan rate in V s−1, R is the gas constant (8.314 J mol−1 K−1), and T is the temperature in K. Thus, Ip of the two reduction peaks R1 and R2 at ∼2.2 and ∼1.9 V vs. Li+/Li, respectively, and the oxidation peak O3 at 2.4 V vs. Li+/Li, were analysed as a function of ν1/2.46 The linear fit of the obtained plots allows the determination of the slope for the calculation of DLi+ (Fig. S5, ESI†). The obtained values are summarized in Fig. S6 and Table S2 (ESI†). In all the analysed cells, DLi+ exhibits the highest value in correspondence of the reduction peak R1 at 2.2 V vs. Li+/Li and decreases at the second discharge step associated with peak R2 at 1.95 V vs. Li+/Li (Fig. S6 in the ESI†). This behaviour can be ascribed to the presence of a high concentration of soluble species with high ionic mobility, such as long-chain polysulfides, at R1. On the contrary, at R2, the most abundant species are short-chain polysulfides, which exhibit low solubility and low ionic mobility. The obtained data reveal that, compared to the pristine Celgard, all the COF-modified separators increase DLi+ due to the confined transportation of Li+ within the one-dimensional (1D) channels featured by COF structures.55 However, among the investigated LSBs, the highest DLi+ values were obtained in the cell based on the KS60@Celgard separator (1.6 × 10−7 cm2 s−1 at 2.2 V vs. Li+/Li). This result suggests that KS60@Celgard allows selective sieving of Li+.56
Electrochemical impedance spectroscopy measurements were further conducted on new cells in the 500 kHz to 100 mHz frequency range at the open circuit voltage (OCV) state, before the first CV cycle and after each CV cycle recorded at a voltage scan rate of 0.1 mV s−1 (Fig. 2e–h). The resulting Nyquist plots were used to gain information on the charge transfer processes at the electrode/electrolyte interface. As shown in Table S3 in the ESI,† all the Nyquist plots were fitted with an appropriate equivalent circuit based on the following circuit elements: Re, representing the electrolyte resistance and general series resistances; Ri and Ci (or Qi), representing the resistance and capacitance (or constant phase element, CPE) related to the charge transfer processes at the electrode/electrolyte interface; an additional RwQw element at low frequency associated with the semi-finite diffusion of Li+, and a final Qdiff element, representing a CPE associated with the diffusion processes of redox species.46,57 The EIS response substantially varies moving from the initial OCV state to the end of CV cycling. For all the studied LSBs, the total Rtot, given by the sum of the various resistances, decreases drastically. Interestingly, Rtot reaches values as low as 6.1 ± 0.1 and 6.2 ± 0.2 Ω in the case of the cells based on KS60@Celgard and K60@Celgard separators, respectively, after 5 CV cycles. Furthermore, the phase angle Bode plot, shown in Fig. S7 (ESI†), provides insight into the Li+ diffusion processes occurring in the cells. In particular, more negative values of phase angle in the low frequency region indicate rapid Li+ diffusion.58 The battery based on the KS60@Celgard separator reaches the most negative phase angle of −51° at 0.1 Hz, while the use of Celgard, K60@Celgard and KS80@Celgard separators results in higher values, i.e. of −21°, −22° and −43°, respectively. Considering that the investigated cells differ only in the composition of the separator coating, these data indicate that the KS60@Celgard separator can efficiently ensure optimal Li+ diffusion, outperforming the other separators.56,58 The combination of EIS and CV data supports that the KS60@Celgard separator is the most efficient one in enabling selective Li+ sieving.
The effect of the different separators on the LSB performances was then studied through GCD measurements. Fig. 3a shows the GCD profiles recorded at C10 rate (1C = 1672 mA gS−1) for LSBs based on the investigated separators (average sulphur loading ∼2 mg cm−2 and E/S ratio = 15 μL mgS−1). The GCD profiles are reported after 3 GCD cycles to ensure that the cells were sufficiently activated by appropriate electrode formation processes, allowing a reliable comparison of their performances. For all the investigated cells, it is possible to distinguish the two voltage plateaus, at ∼2.3 and ∼2.1 V, typically displayed by LSBs during their discharge. This discharging behaviour is well reversed during the charging step. The plateau at the highest voltage is generally associated with the formation of long-chain polysulfides (Li2Sx, 4 ≤ x ≤ 8), which are then reduced to low-order insoluble Li2S2 and Li2S during the second voltage plateau.59,60 The cells based on Celgard, KS60@Celgard, K60@Celgard and KS80@Celgard separators show an initial specific discharge capacity of 879, 1050, 1072 and 906 mA h gS−1, respectively. Interestingly, all the COF-modified separator coatings induced an increase of the specific discharge capacity compared to the cell based on pristine Celgard. Thus, at low C-rate, the specific discharge capacity is highly influenced by the ability of the separator to trap high-order polysulfides: the presence of the COF porous structures ensures efficient polysulfide trapping, leading to high coulombic efficiency for the LSB conversion processes, without compromising Li+ transport (see EIS and CV analyses).61–63 This evidence can be explained by the presence of additional pore channels in the COF structures. New diffusion pathways in the modified separators can effectively hinder and retard the polysulfide migration and shuttle, with a positive effect on the Li+ transport in the rest of the separator, and thus, on the overall electrochemical performance of the cell.2 Scan rate-dependent CV analysis demonstrated that the COF-modified separators, in particular KS60@Celgard, can promote the diffusion of Li+ (see Fig. 2a–d). In particular, polysulfide diffusion is affected by the chemical environment in the COF nanochannels.32 Compared to polysulfides, Li+ is less sterically hindered and positively charged. Thus, it can rapidly diffuse in the COF pores.43,64 Furthermore, the cell overpotentials at the second discharge plateau are 130, 140, 220 and 170 mV for the cells containing pristine Celgard, KS60@Celgard, K60@Celgard and KS80@Celgard separators, respectively. Low values of overpotential can be associated with the efficient conversion of the long-chain polysulfides.53 The data clearly indicate that COF KS1 facilitates polysulfide conversion processes, essentially acting as a catalyst for these reactions. Conversely, COF K1 seems to primarily function as a polysulfide retainer. Notably, a high content of COF KS1 on the separator causes an increase of the cell overpotential and a decrease of the cell capacity. Based on the previous CV and EIS analyses, an excessive content of COF KS1 can decrease DLi+ and, thus, the total charge transfer resistance and the specific discharge capacity of the corresponding cell.
Fig. 3b–e display the rate capability of the investigated LSBs, screening C-rates from C10 to 1C. Table S4 in the ESI† lists the specific discharge capacity measured at each C-rate. At low C-rate, the cells with the COF-modified separators displayed higher specific discharge capacities (i.e., 933, 1028, 733 mA h gS−1 for KS60@Celgard, K60@Celgard and KS80@Celgard separators at C8) compared to the cell based on pristine Celgard (704 mA h gS−1 at C8), thanks to their ability to efficiently trap the long-chain polysulfides, thus, ensuring high S utilization. By increasing the C-rate, significant differences can be detected between the performances of cells based on different COF-modified separators. In particular, at 1C, the use of K60@Celgard and KS80@Celgard separators substantially reduces the specific discharge capacities to 44 and 150 mA h gS−1, respectively. In fact, at high C-rate, the capacity is strongly affected by the Li+ transport.61,62 Although K60@Celgard and KS80@Celgard separators can efficiently alleviate the polysulfide shuttle, they also slow down the transport of Li+, as proved by the phase angle Bode plot and DLi+ analyses. The use of the KS60@Celgard separator ensures high specific discharge capacities at all the investigated C-rates, confirming a dual functional role of KS COF as a polysulfide retainer and a Li+ sieve. Another important parameter for the LSBs is the discharge capacity loss, calculated from the discharge capacity ratio among the last discharge of the first and last GCD cycles acquired at C10. The discharge capacity loss is 17.5%, 6.4%, 0.3% and 15.5% for the cell based on pristine Celgard, KS60@Celgard, K60@Celgard and KS80@Celgard separators, respectively, indicating a satisfactory cyclability for the investigated LSBs, whose structural integrity is therefore preserved even after high-rate operation.65
Fig. 4 and S8 (ESI†) show the complete stability test and selected GCD profiles measured at C5 over 190 GCD cycles for the LSBs based on pristine Celgard, KS60@Celgard, K60@Celgard and KS80@Celgard separators, respectively. The measurements were performed after cell activation at low C-rates to ensure reproducible behaviours. For the cell based on pristine Celgard, the specific discharge capacity decreased significantly in the first GCD cycles, until stabilizing after ca. 20 GCD cycles. After the same number of GCD cycles, the specific discharge capacities of the cells based on KS60@Celgard and K60@Celgard separators reached their maximum values. This behaviour can be associated with the prolonged diffusion pathway from the cathode to the anode side when the functional COF coating is added to Celgard.2 All the batteries displayed excellent cyclability for 190 GCD cycles with an average oulombic efficiency between 98 and 99%. The most performant cell based on KS60@Celgard (sulphur loading of 2.4 mgS cm−2) has shown the highest specific discharge capacity of 850 mA h gS−1 with 74.1% retention of its maximum specific discharge capacity after 190 GCD cycles.
![]() | ||
| Fig. 4 Specific discharge capacity and coulombic efficiency over 190 GCD cycles at C5 measured for LSBs based on pristine Celgard, KS60@Celgard, K60@Celgard and KS80@Celgard separators. | ||
Overall, the high specific discharge capacity at all the investigated C-rates, the capacity retention and coulombic efficiency of the cell based on the KS60@Celgard separator are explained by the ability of this separator to adsorb polysulfides and electrocatalytically promote the conversion of sulphur species, alleviating the shuttle effect and excessive conversion reaction overpotentials.66 Based on literature data, Table S5† reports the comparison between the performances of different LSBs based on COF-based functional separators. Notably, this analysis evidences that most of the investigations on LSBs at the laboratory scale are performed using cathodes with low sulphur loading below 2 mgS cm−2, leading to low absolute energies that are not adequate for practical cells,67,68 although resulting in higher specific discharge capacities compared to those reported in our work. Considering the high sulphur loading used in the present study, we believe that the performances of the fabricated LSBs, achieved with flat current collectors, are significant in the field.
:
5, 1
:
2, 1
:
4 and 1
:
4 for pristine Celgard, KS60@Celgard, K60@Celgard and KS80@Celgard separators, indicating that the redox reversibility of the different species depends on the characteristics of the separator.73,74 The KS60@Celgard separator ensures the highest atomic ratio of S species corresponding to S8 and Li2Sx, demonstrating its electrocatalytic activity towards the LSB conversion processes, enabling an efficient oxidation of Li2Sx to S8.12
Additionally, morphological post mortem analysis was conducted on both Li anodes and separators by means of SEM measurements. It is well known that the shuttle of polysulfides corrodes the Li metal anode, leading to the depletion of active Li and exacerbating unevenness in the anode.75 Once polysulfides diffuse to the anode side due to concentration gradients, they can rapidly react with the Li anode, forming insoluble species such as Li2S at the solid electrolyte interface (SEI).
This process contributes to increased SEI inhomogeneity, uneven Li plating/stripping and the formation of Li dendrites. Ultimately, the reaction between polysulfides and dendritic Li damages the original anode structure and yields inactive Li.75–77 Fig. S9† shows the smooth surface of a standard fresh Li anode, while the comparison with those extracted from the cycled LSBs containing pristine Celgard, KS60@Celgard, K60@Celgard and KS80@Celgard separators is reported in Fig. 5e–h. In all cases, the anode surface morphology normally differs from the fresh Li because of repeated Li plating/stripping occurring during long-term GCD cycling. In particular, when the pristine Celgard separator is used, the Li anode evidences a highly inhomogeneous surface, with the deposition and growth of a large number of Li dendrites along with pits on the anode surface (Fig. 5e).78,79 Differently, for the anodes of the LSBs based on KS60@Celgard, K60@Celgard and KS80@Celgard separators, the Li deposited after subsequent GCD cycles forms more uniform layers, especially when KS1 COF is used, without visible Li dendrite formation (Fig. 5f–h). Thus, the morphological post mortem analysis provides evidence that the modification of the separator by COF-based coatings reduces the polysulfide shuttle, which, in turn, mitigates the corrosion of the Li anode. Additionally, Fig. S10† shows that Li dendrites accumulated in the pristine Celgard separator, while no morphological modification occurred on KS60@Celgard, K60@Celgard and KS80@Celgard separators.
:
Li2Sx content ratio, as confirmed by the ex situ post mortem XPS analysis of the separators, obtained by disassembling charged LSBs after 190 GCD cycles. These results demonstrate that the shuttle effect mitigation is accompanied by an efficient oxidation of Li2Sx to S8 (electrocatalytic effect), i.e., high sulphur utilization. In parallel, the equivalent separator modified with a coating based on 60 wt% COF K1, carrying a phenyl linker, results in LSBs with a specific discharge capacity of 599 mA h gS−1, while the use of a higher content (80 wt%) of KS1 COF in the separator reduces the performances of the corresponding LSB (e.g., specific discharge capacity of 577 mA h gS−1), under the same operating conditions (C5). Additionally, post mortem SEM analysis on the Li anodes recovered after cycling indicates that, differently from the case of pristine Celgard, the KS60@Celgard separator significantly mitigates polysulfide shuttle, as proved by the absence of Li dendrite growth. Overall, electrochemical investigations and ex situ post mortem XPS and SEM analyses elucidated the correlation between the nature of the linker in the COF structure, the overall COF content in the separator and the performance of LSBs based on COF-modified Celgard separators. Overall, this work casts light onto the cooperativity among the polysulfide retention, the selective Li+ sieving and the electrocatalytic properties of COF-modified Celgard separators for LSBs, paving the way towards the use of layered porous materials in high-performance LSBs.
Footnote |
| † Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4ta03930k |
| This journal is © The Royal Society of Chemistry 2024 |