Qiyin
Chen
ab,
Yun
Hu
c,
Jie
Lin
c,
Jingsong
Huang
*c,
Shu-Ling
Gong
*a and
Guohua
Xie
*ab
aSauvage Center for Molecular Sciences, Hubei Key Lab on Organic and Polymeric Optoelectronic Materials, Department of Chemistry, Wuhan University, Wuhan 430072, China. E-mail: gongsl@whu.edu.cn; ifeghxie@xmu.edu.cn
bThe Institute of Flexible Electronics (Future Technologies), Xiamen University, Xiamen 361005, China
cOxford Suzhou Centre for Advanced Research (OSCAR), University of Oxford, Suzhou 215123, China. E-mail: jingsong.huang@oxford-oscar.cn
First published on 4th January 2024
Interfacial modification is vital to boost the performance of colloidal quantum-dot light-emitting diodes (QLEDs). We introduce phenethylammonium bromide (PEABr) as an interlayer to reduce the trap states and exciton quenching at the interface between the emitting layer (EML) with CdSe/ZnS quantum-dots and the electron transport layer (ETL) with ZnMgO. The presence of PEABr separates the EML and the ETL and thus passivates the surface traps of ZnMgO. Moreover, the interfacial modification also alleviates electron injection, leading to more improved carrier injection balance. Consequently, the external quantum efficiency of the PEABr-based red QLED reached 27.6%, which outperformed those of the previously reported devices. Our results indicate that the halide ion salts are promising to balance charge carrier injection and reduce exciton quenching in the QLEDs.
New conceptsQuantum-dot light-emitting diodes (QLEDs) possess high efficiency, high brightness, and wide color gamut, which makes them one of the most promising candidates for active matrix displays. Normally, the hole transporting layer, the emitting layer, and the electron transporting layer are consecutively solution-processed to construct QLEDs. Nevertheless, it is tricky to maximize the electroluminescent performance due to charge imbalance and interfacial defects in the solution-processed devices. In this communication, we managed to passivate the interface between the quantum-dot emitting layer and the commonly used electron transporting layer ZnMgO by introducing phenethylammonium bromide (PEABr), which is one of the ingredients used in perovskite LEDs and solar cells. Based on all-spin-coating procedures, the trap density was significantly reduced from 1.1 × 1018 cm−3 (control device) to 5.9 × 1017 cm−3. More importantly, the charge balance was improved simultaneously, resulting in the record high external quantum efficiency of 27.6%, and the considerably low turn-on voltage of only 1.8 V. |
In order to address these aforementioned issues related to ZnO, researchers have developed several strategies, including the passivation and chemical doping of the ZnO-based ETL, interfacial modification, device engineering, and ligand modification of QDs.15–20 Among these strategies, interfacial modification is one of the most cost-effective methods and widely employed in optoelectronic devices, such as organic light-emitting diodes (OLEDs), organic solar cells (OSCs), perovskite light emitting diodes (PeLEDs), and perovskite solar cells (PSCs).9,21–24 For example, Tang et al. modified the interface between the perovskite EML and the ZnMgO ETL with the amino-based compound, which not only interacted with ZnMgO and thereby modified the growth of perovskite film, but also passivated the perovskite defects.25 Tulus et al. fabricated the ZnO-based PSCs with the interlayer C60, which passivated the interfacial trap states and reduced non-radiative recombination losses, resulting in the increased efficiency and stability.26 Soultati et al. inserted a thin organic layer between the ZnO ETL and the photoactive layer in the nonfullerene-based OSCs.27 It reduced the work function of ZnO, improved the electron transport, and increased the degree of crystallization of the photoactive layer. As a result, the photostability and power conversion efficiency of OSC devices were significantly improved.
Since the universality of interfacial modification has been demonstrated in different ZnO-based optoelectronic devices, many interfacial materials, such as PMMA, PVPy, Al2O3, PEIE and Cs2CO3, have been introduced into QLEDs to improve the EL performance.5,28–31 For instance, Dai et al. inserted an ultrathin insulating layer PMMA at the ZnO/QDs interface to reduce the interaction between ZnO and QDs, and obtained a high external quantum efficiency (EQE) of 20.5%.5 Yun et al. used the non-conjugated polymer PVPy as the interlayer in the inverted QLEDs to efficiently block the leakage current.28 Qiu et al. fabricated the QLEDs with Cs2CO3 to inhibit the interaction between ZnO and QDs and passivate the defects on the surface of QDs. Finally, the current efficiency was improved from 10 to 32 cd A−1.31
In this contribution, we introduced a halide ion salt, phenethylammonium bromide (PEABr), as the interfacial modification layer inserted between the CdSe/ZnS-based EML and the ZnMgO ETL. The outstanding EQE of 27.6% was demonstrated, due to the balanced charge carrier injection and reduced exciton quenching. To our knowledge, this is the highest EQE of the CdSe/ZnS-based red QLEDs ever reported. The photoluminescence (PL) and time-resolved photoluminescence (TRPL) results indicated that PEABr could passivate the surface traps of ZnMgO and suppress interfacial exciton quenching, simultaneously. The measurements of the transient electroluminescence (TREL) and the electron-only device (EOD) confirmed the improved balanced carrier injection and the reduced interfacial trap density in the presence of PEABr.
The TRPL was recorded to unravel the role of PEABr. The TRPL spectra of QDs, QDs/PEABr/ZnMgO, and QDs/ZnMgO, shown in Fig. 1e, rendered the average fluorescence lifetimes (τavg) of 23.8, 22.3 and 20.2 ns, respectively. The τavg of QDs/PEABr/ZnMgO was longer than that of QDs/ZnMgO, slightly shorter than that of the pristine QDs. The prolonged fluorescence lifetime resulted from the separation of the QDs and ZnMgO. As confirmed by Fig. 1f, the PL intensity of ZnMgO was significantly reduced when ZnMgO was deposited on PEABr. Since the emission of ZnMgO in the visible wavelength range is ascribed to the surface traps,32–34 it suggests that PEABr can effectively passivate the surface traps of ZnMgO. Combining these PL and TRPL results, it is clear that the fluorescence quenching of the QDs/ZnMgO film was caused by the surface traps of ZnMgO, which can be easily passivated by PEABr.
Fig. S1 (ESI†) presents the atomic force microscopy (AFM) images of the ZnMgO films deposited on the QDs with and without PEABr. Both films displayed comparatively small root mean square (RMS) roughness values of 2.07 and 2.05 nm, respectively. Obviously, the similar RMS values indicate that PEABr has no negative influence on the surface morphologies of ZnMgO.
To evaluate the influence of PEABr on the EL performance of the QLEDs, devices with the structure of anode/hole injection layer (HIL)/hole transport layer (HTL)/EML/interfacial modification layer (IML)/ETL/cathode were constructed, where the anode/cathode were ITO and Al, respectively. PEDOT:PSS, TFB, red emissive CdSe/ZnS QDs, PEABr, and ZnMgO NPs served as the HIL, HTL, EML, IML, and ETL, respectively. The control device without the IML was fabricated in the same run as a reference. The schematic diagram of the PEABr-based device structure is shown in Fig. 2a. Firstly, we compared the EL performance of the devices with different spin-coating speeds, i.e., 1000, 2000, and 3000 rpm, and thereafter two different annealing temperatures (50 °C and 80 °C) of the PEABr layer. The corresponding current density–voltage–luminance (J–V–L), current efficiency (CE), power efficiency (PE), and EQE curves are shown in Fig. S2 and S3 (ESI†) and the key EL paraments are summarized in Tables S1 and S2 (ESI†), respectively.
Later, the optimized fabrication conditions of the PEABr layer were determined with a spin-coating speed of 2000 rpm for 40 s, a fixed acceleration of 1500 rpm, and an annealing temperature of 50 °C for 10 min. In parallel, the corresponding control device was fabricated. The normalized EL spectra of the control and PEABr-based devices under a voltage of 3 V are shown in Fig. 2b. Both devices exhibited identical emission peaking at 628 nm with a narrow FWHM of 24 nm (Table 1). The corresponding to Commission International de I’Eclairage (CIE) color coordinates were (0.68, 0.31). Fig. 2c shows the J–V–L curves of both devices. It is obvious that the current density of the PEABr-based device is lower than that of the control device, which indicates that the presence of PEABr might retard the carrier injection. Also, from the J–V curves of both devices, we obtained the ideality factor (eqn (1)) by fitting them based on the diode model equation.35
(1) |
Device | V on (V) | λ EL (nm) | FWHMc (nm) | PEd (lm W−1) | CEe (cd A−1) | EQEf (%) | CIEg (x, y) |
---|---|---|---|---|---|---|---|
a Turn-on voltage at a luminance of 1 cd m−2. b Peak wavelength of the EL spectrum. c Full-width at half-maximum of the EL spectrum. d Maximum power efficiency. e Maximum current efficiency. f Maximum external quantum efficiency. g Commission International de I’Eclairage color coordinates. | |||||||
Control | 1.8 | 628 | 24 | 31.9 | 26.6 | 20.1 | (0.68,0.31) |
PEABr | 1.8 | 628 | 24 | 43.9 | 36.6 | 27.6 | (0.68,0.31) |
The fitted results reveal that the ideality factor of the PEABr-based device is 4.77. Meanwhile, it is 5.16 for the control one. The lower value of the ideality factor evidences the better diode characteristics. Since both devices share the same hole injection, it is supposed that PEABr alleviates the electron injection and results in a more balanced charge injection in the PEABr-based device. Derived from the luminance curves, both devices exhibited a low turn-on voltage of 1.8 V at a luminance of 1 cd m−2. As shown in Fig. 2d and e, the PEABr-based device exhibited a significantly higher CE and EQE, compared with the control device. The PEABr-based device achieved the maximum EQE, PE, and CE of 27.6%, 43.9 lm W−1, and 36.6 cd A−1, respectively. In contrast, these values of the control device were much inferior, i.e., EQE = 20.1%, PE = 31.9 lm W−1, and 26.6 cd A−1, respectively. It is worth noting that the EQE of the PEABr-based device remained much higher than that of the control device over a wide range of luminance, from 100 to ca. 20000 cd m−2. To the best of our knowledge, such EL characteristics of the PEABr-based device outperformed any other CdSe/ZnS-based red QLEDs. A comparison of the state-of-the-art QLEDs is shown in Table 2.1,2,36–41 In addition, the devices were easily reproduced, evidenced by the EQE distribution shown in Fig. 2f.
Structure | λ EL (nm) | FWHMb (nm) | EQEconc (%) | EQEmodd (%) | Ref. |
---|---|---|---|---|---|
a Peak wavelength. b Full-width at half-maximum of the EL spectrum. c Maximum external quantum efficiency of the control device. d Maximum external quantum efficiency of the modified device. N.A.: not available. | |||||
ITO/PEDOT:PSS/PVK/QD:TAPC/ZnO/Al | 628 | 28 | 11.8 | 15.7 | 36 |
ITO/ZnO (LZO)/QD/TCTA/NPB/HAT-CN/Ag | 621 | 24 | 12.6 | 16.4 | 37 |
ITO/rGO/PEDOT:PSS/PVK/QDs/ZnO/Al | 630 | 21 | 7.9 | 17.3 | 40 |
ITO/PEDOT:PSS/TFB/QDs/ZnO/Al | 628 | 20 | 14.3 | 17.4 | 38 |
ITO/PEDOT:PSS/TFB/QDs/ZnMgO/Ag | 630 | N.A. | 16.5 | 19 | 1 |
ITO/ZnO/PEIE/QDs/PVK/PEDOT:PSS/Al | 624 | 32 | 20.7 | N.A. | 39 |
ITO/PEDOT:PSS/TFB (PVK, PTAA, and Poly-TPD)/QD/ZnO (ZnMgO)/Ag | 618 | N.A. | 6.5 | 21.1 | 2 |
ITO/PEDOT:PSS/TFB-PVK/QDs/ZnMgO/Ag | 628 | N.A. | 17.6 | 22.7 | 41 |
ITO/PEDOT:PSS/TFB/QDs/PEABr/ZnMgO/Al | 628 | 24 | 20.1 | 27.6 | This Work |
To clarify the role of PEABr in modulating the carrier and exciton dynamics, TREL measurements were conducted. Fig. 3a represents the rising part curves of the devices when applying a pulsed voltage of 3 V. Since the devices shared the same HTL, the slightly delayed switch-on of the EL intensity of the device with PEABr might be attributed to the reduced electron injection (see Fig. 3a), driven by a voltage pulse of 3 V. Combining the J–V–L curves of both devices, we speculate that PEABr preferred to improve the charge carrier balance by alleviating the injection of electrons. Based on the TREL curves shown in Fig. 3b, the decayed lifetime of the control device (4.04 μs) is shorter than that of the PEABr-based device (12.72 μs), which implies that excitons in the control device suffered from more severe quenching than that in the PEABr-based device. This is well consistent with the TRPL behaviors shown in Fig. 1e.
To further study the effect of PEABr modification on carrier injection, we investigated the capacitance–voltage (C–V) characteristics of the PEABr-based device and the control one at a fixed frequency of 10 kHz (see Fig. 4a). The geometric capacitance values of both devices are almost constant at 3.3 nF under a low bias voltage <0.5 V. Then the values rise because of the fast carrier injection and decrease significantly after 2.4 V due to the intensive radiative recombination. Since the hole injection would be identical for both devices, the variation of the C–V curves should be attributed by electron injection. The lower capacitance after the turn-on of the PEABr-based device demonstrates that PEABr reduced the excessive electron injection and decreased the accumulation of electrons in the PEABr-based device. It is clear that the current density of the PEABr-based device was lower than that of the control device while both devices shared the same hole injection (see Fig. 2c). Meanwhile, the J–V curves of the EODs exhibited the same trend, that the PEABr-based EOD had a lower current density when PEABr was inserted (see Fig. 4b). Furthermore, the similar voltages at the peak capacitance of both devices also indicate that in both devices the built-in potential (Vbi) was barely changed, in the presence of PEABr.
Fig. 4 (a) Capacitance–voltage curves of the control and the PEABr-based QLEDs. (b) J–V curves of the EODs with and without PEABr. |
The interfacial trap density is an important parameter to manifest the effect of interfacial modification, which can be simply calculated from the J–V curve of the single-carrier device. Therefore, we fabricated the EODs with the structures of ITO/ZnMgO (60 nm)/QDs (25 nm)/PEABr (5 nm)/ZnMgO (60 nm)/Al (100 nm) (named PEABr-based EOD) and ITO/ZnMgO (60 nm)/QDs (25 nm)/ZnMgO (60 nm)/Al (100 nm) (named control EOD), respectively. Based on the J–V curves of both EODs shown in Fig. 4b, the intrinsic interfacial trap density (eqn (2)) can be calculated by the following equation.42
(2) |
The VTFL values were determined to be 0.54 and 0.99 V for the PEABr-based and control EODs, respectively. It is found that the PEABr interlayer reduces the interfacial trap density from 1.1 × 1018 cm−3 (control device) to 5.9 × 1017 cm−3. The low Nt mainly originated from the reduced traps passivated by PEABr. This would lead to weaker exciton quenching, which is consistent well with the steady-state PL and TRPL results.
Based on the above-mentioned measurements and characterization, it is deduced that PEABr as the interfacial modification layer not only is beneficial to reduce the trap density and thus suppress exciton quenching, but also helpful to improve carrier injection balance, which plays a vital role in boosting the EL performance.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3nh00495c |
This journal is © The Royal Society of Chemistry 2024 |