Redox-active oxide-molten salt composites as a new family of high-capacity thermal energy storage materials

Hilal Bektas a, Runxia Cai a, Saqlain Raza b, Jun Liu b and Fanxing Li *a
aDepartment of Chemical and Biomolecular Engineering, North Carolina State University, 911 Partners Way, Raleigh, North Carolina 27695, USA. E-mail: fli5@ncsu.edu
bDepartment of Mechanical and Aerospace Engineering, North Carolina State University, Raleigh, North Carolina 27695, USA

Received 22nd March 2025 , Accepted 21st May 2025

First published on 21st May 2025


Abstract

This study introduces a new family of redox-active oxide-molten salt (ROMS) composites for high-capacity thermal energy storage. Porous perovskite oxides serve as active support materials, facilitating thermochemical energy storage through redox reactions, while latent heat from the phase change of the salt mixture enables high energy density within a narrow temperature swing. We demonstrated the compatibility between perovskites and salt mixtures, with 12 out of 25 tested combinations proving successful. The diverse properties of perovskites and salt mixtures resulted in ROMS compositions with different functionality and performance, three of which are highlighted in this work. La0.8Sr0.2FeO3−δ:NaF–CaF2–LiF exhibited excellent latent heat-based energy storage as well as long-term stability with a total capacity of ∼530 kJ kg−1 (510–660 °C). Sr0.125Ca0.875Fe0.25Mn0.75O3−δ:NaF–CaF2 achieved the overall energy density of ∼523 kJ kg−1 (670–820 °C) through both phase-transition and redox-based mechanisms, though gradual deactivation was observed over long-term operation. Lastly, La0.8Sr0.2FeO3−δ:Li2MoO4, a highly redox-active ROMS composition, delivered up to 875 kJ kg−1 when applied for waste heat recovery from fuel-containing exhaust gas streams.


1. Introduction

The combustion of fossil fuels, which accounts for approximately 80% of the world's energy utilization, stands as the predominant contributor to greenhouse gas emissions.1–3 Meanwhile, only less than half of the energy derived from fossil fuels is converted into useful forms such as electric power, with the rest being discharged as waste heat.4 Other energy-intensive industries such as iron and steelmaking also produce vast amounts of high-grade heat (>500 °C), with processes like electric arc furnaces or coke ovens generating exhaust gas at high temperatures.5,6 As such, capturing the excess heat for industrial applications or power generation would significantly improve the energy efficiency of the processes and substantially reduce the carbon emissions.4,5,7 However, the recovery of waste heat faces challenges due to the mismatch between the operational requirements of energy supply and demand.4 Also, the intermittency or fluctuations of many heat sources restrict the continuous operation of the waste heat recovery system.8,9 Thermal energy storage (TES) can overcome these challenges by adapting to the properties of high-temperature heat sources.10–12 A cost-effective thermal energy storage system can capture the energy from the heat source, and store and release it on demand for industrial processes or power generation.12,13

TES can find applications in the forms of sensible, latent, and thermochemical heat. Among these, sensible heat storage materials have been most widely investigated and commercially mature owing to their simplicity.13,14 Molten nitrate salts are the most commonly used sensible heat storage materials for medium (200–400 °C) to high (>400 °C) temperature TES, often employed as heat transfer fluids due to their favorable characteristics such as high heat capacity and low melting point.15,16 For example, LiNO3–NaNO3–KNO3–Ca(NO3)2, extensively studied for sensible heat storage application, has been utilized as heat transfer fluid in solar parabolic systems.11,17,18 Nitrate salts can provide energy storage densities ranging from 100 to 500 kJ kg−1 but they require large temperature swings of ∼300 °C to achieve the high values.13,19,20 In addition, the relatively low decomposition temperatures of molten nitrate salts limit their applicability for temperatures exceeding 560 °C.13

Compared to sensible heat storage materials, latent heat storage systems that rely on phase change materials (PCM) exhibit notable advantages, primarily due to their superior energy storage density, which requires low volume and operates within a narrow temperature range.11,12 For medium- and high-temperature (200–1400 °C) applications, fluoride, and carbonate-type molten salts are particularly attractive phase-change materials (PCM) for latent heat storage with their considerably large heat of fusion.21 They are suitable for use at operating temperatures above 500 °C due to their high melting points. However, the application of molten salts is restricted by thermal instabilities above the melting point. Besides, the melting and solidification of PCMs cause handling difficulties in fluidized beds or single-tank systems. The corrosive nature of molten salts imposes additional limitations on their applications in heat storage.13,22

To address the above-mentioned challenges, there has been growing interest in form-stable composite materials consisting of PCMs and supporting materials in recent years.10,11,23–27 Form-stable composite materials enclose the PCMs within a skeleton material and reduce the leakage of PCMs.24 Various supporting materials, such as diatomite,25,28,29 vermiculite,26 magnesium oxide,23 and expanded graphite,30 have been used to fabricate the composite materials. Among them, diatomite has attracted more interest owing to its high porosity, corrosion resistance, and low cost.10,25 For example, Jiang et al. used a porous modified diatomite-based skeleton material to improve the thermophysical properties of NaNO3.25 They obtained a total energy storage density of 382.92 kJ kg−1 in the operating temperature range of 130–330 °C with 58.67 wt% salt loading and improved the micro-flow of molten salt within the large pores of the modified diatomite. Li et al. studied sodium nitrate-expanded vermiculite (EV) composite materials, achieving a latent heat of 157.2 kJ kg−1, and a high salt[thin space (1/6-em)]:[thin space (1/6-em)]EV ratio of 734.6 wt% (defined as adsorptive capacity) using the direct impregnation method.26 Jiang et al. developed a form-stable composite material using LiNO3–NaNO3–KNO3–Ca(NO3)2 and calcium silicate with a melting point of 103.5 °C and latent heat of 73.59 kJ kg−1.11 The high porosity of calcium silicate played a vital role in preventing salt leakage by absorbing large amounts of nitrate salt, thus ensuring the long-term stability of over 1000 thermal cycles. While these studies have mainly focused on low (<200 °C) and medium temperatures (200–400 °C) applications due to the low melting point of nitrate salts, efforts have been made to extend the operating temperature range to high temperatures (>400 °C). Qian et al., for instance, introduced a group of composite materials consisting of polyethylene glycol, LiNO3, and Na2SO4 which were aimed to be used in low, middle, and high-temperature energy storage, respectively.24 Furthermore, Ge et al. also proposed a composite material for the medium and high temperature ranges, by using LiCO3–NaCO3 as the PCM, MgO as the ceramic support material, and additionally carbon nanotubes as the thermal conductivity enhancer.23 Their studies emphasized the significance of good wettability of the salt with ceramic material to ensure the formation of a robust composite material. Although the proposed composite materials offer promising properties and prevent salt leakage, inert support materials limit the energy efficiency of such composites, necessitating a large temperature swing for effective heat storage.

Alternatively, thermochemical energy storage (TCES) has recently gained significant attention owing to its potential for achieving high energy density in wide operating temperature ranges and extended durations.19,31 Particularly, TCES systems, which utilize the chemical energy of reversible redox reactions of metal oxides, have been widely studied in recent years.32,33 Within the realm of redox-active metal oxide materials, perovskite oxides with the general formula of ABO3 (where A is typically an alkali, alkaline earth, or a lanthanide metal cation and B is a transition metal cation) have shown considerable advantages over conventional redox materials.34,35 They have the ability to continuously exchange their lattice oxygen over a wide range of temperatures and partial oxygen pressures, facilitating thermochemical energy storage under flexible operating conditions.36,37 Conversely, the redox reactions of monometallic oxides are discrete and restricted to specific high temperatures.32 Furthermore, the flexible structures of perovskite oxides enable tailorable thermochemical properties, allowing them to be utilized in various energy storage applications.38 The excellent kinetics of perovskites, attributed to their high lattice oxygen diffusion rate, further enhances their utility.33,39 To date, perovskite oxides have demonstrated TCES densities ranging from 34 to 571 kJ kg−1-ABO3 with an operating temperature window extending up to 1250 °C.34–47 However, they require large temperature and oxygen partial pressure swings to achieve such densities, thereby limiting the energetic efficiency of the processes.

To address the limitations of existing TES materials, this study reports a new class of materials, i.e. redox-active oxide-molten salt (ROMS) composites, which combine molten salts and perovskite oxides in a dual-phase composite structure.48 In these composites, the latent heat storage from the phase change of molten salts serves as the primary energy storage mechanism, while redox-active oxide materials act as supporting structures to prevent salt leakage and contribute additional thermochemical energy density through redox reactions. ROMS composites offer several potential advantages: (1) the oxide exoskeleton stabilizes the molten salt via favorable surface tensions, similar to non-redox-active composites;27 (2) the latent heat storage of molten salts narrows the temperature swing required for redox-based energy storage; (3) both perovskite oxides and molten salts are highly tunable, enabling compatibility with a range of operating conditions; and (4) the high redox activity facilitates efficient recovery of waste heat from fuel-containing exhaust streams. This study demonstrates the compatibility of perovskite oxides and salt mixtures as energy storage media, highlighting three compositions with varying features that cater to different application scenarios ranging from thermal energy only to high-temperature fuel containing flue gas.

2. Experimental methods

2.1 Material preparation

The abbreviations and synthesis methods of metal oxides that were used are listed in Table 1. LSF1 and LSFCo were commercial La0.8Sr0.2Fe0.97O3−δ and La0.8Sr0.2Co0.8Fe0.2O3−δ, respectively obtained from Praxair Surface Technologies while the rest was synthesized either by solid-state or sol–gel method. Detailed descriptions regarding the solid-state method can be found in our previous study.49 The procedure for the sol–gel method is provided in the ESI. Eutectic and ternary salt mixtures were prepared by mixing the salts in a mortar with the specific ratios provided in Table 2. The salts used in this study were LiF (97%), NaF (99%), CaF2 (99%), MgF2 (99%), and KF (99%), from Thermo Fisher Scientific and Li2CO3 (≥99%), Na2CO3 (≥99.5%) NaCl (≥99.5%), and Li2MoO4 (99.9%) from Sigma Aldrich. The composite materials were prepared by using facile mixing and sintering, as illustrated in Fig. 1b. Fig. 1b is adopted to prepare the composites using either as received oxides or the porous oxides prepared viaFig. 1a. Detailed descriptions regarding material preparation for XRD, TGA-DSC tests as well as preparation of pellets for thermal conductivity measurements can be found in the ESI.
Table 1 The abbreviation of metal oxides that were used in composite materials
Sample name Abbreviation Synthesis method
Ca2AlMnO5+δ CAM Sol–gel
SrFeO3−δ SF Ball mill
Sr0.75Ba0.25FeO3−δ SBF Ball mill
Sr0.25Ca0.75Fe0.25Mn0.75O3−δ SCFM1 Sol–gel
Sr0.125Ca0.875Fe0.25Mn0.75O3−δ SCFM2 Sol–gel
Sr0.05Ca0.95Mn0.95Co0.05O3−δ SCMCo1 Ball mill
Sr0.05Ca0.95Mn0.9Co0.1O3−δ SCMCo2 Ball mill
La0.8Sr0.2FeO3−δ LSF1 Commercial
La0.6Sr0.4FeO3−δ LSF2 Ball mill
La0.7Sr0.3FeO3−δ LSF3 Ball mill
La0.3Sr0.7Co0.9Mn0.1O3−δ LSCoM1 Ball mill
La0.7Sr0.3Co0.9Mn0.1O3−δ LSCoM2 Ball mill
La0.8Sr0.2Co0.8Fe0.2O3−δ LSFCo Commercial


Table 2 The ratios and phase change properties of eutectic salts reported in the literature
Salt mixture Weight ratio Heat of fusion (kJ kgsalt−1) Melting point (°C)
a The eutectic point for LiF–NaF was provided with a mole ratio of 0.61–0.39 in the FactSage database, heat of fusion was reported for a ratio of 0.6–0.4 in Phillips et al.’s study.51
Li2CO3–Na2CO3[thin space (1/6-em)]50 0.44–0.56 370 496
LiF–NaF–CaF2[thin space (1/6-em)]51 0.35–0.38–0.26 640 615
NaF–CaF2[thin space (1/6-em)]52,53 0.53–0.47 520–600 810
MgF2–NaF–CaF2[thin space (1/6-em)]52,53 0.14–0.52–0.34 510–540 745–754
NaF–NaCl54 0.26–0.73 572 674
NaF–KF53 0.33–0.67 550–560 721
LiF–CaF2[thin space (1/6-em)]53 0.54–0.46 750–760 766
LiF–NaF[thin space (1/6-em)]51,55 0.49–0.51 816a 649
Li2MoO4[thin space (1/6-em)]56 280 705



image file: d5ta02329g-f1.tif
Fig. 1 Schematic representation of material preparation (a) salt-grinding method for the formation of porous oxide (b) composite material preparation small portion of the composite particles were used for TGA-DSC tests, while the rest was prepared for the XRD analysis.

For the long-term tests, we applied the salt-grinding method to the perovskite oxides to obtain a porous structure before preparing the composite material. Schematic representation of this method is provided in Fig. 1a. The perovskite oxides were mixed with NaCl and 3 mm ZrO2 beads in a stainless-steel sample jar with a specific mass ratio. The jar was ball milled at 1200 rpm for 24 h using a high-energy ball mill. The resulting mixtures were rinsed with distilled water to remove NaCl using the centrifuge tube for 8 min at 6000 rpm. This rinsing step was repeated 3 times. Afterward, the remaining wet particles were dried in a vacuum oven at 80 °C for 30 min and then at 130 °C overnight. BET surface area, pore width, and volume of LSF1 were determined using a Micromeritics ASAP 2020 instrument. First, the samples were degassed at 200 °C for 10 hours to get rid of the adsorbed species on the surface. After that, nitrogen adsorption isotherms were obtained in the relative pressure range (P/P0) of 0.01–1 at 77 K.

2.2 Characterization

We characterized the crystal structures of the composite materials using an Empyrean PANalytical XRD with Cu-Kα radiation (λ = 1.5406 Å) at an operating voltage of 45 kV and a current of 40 mA. XRD patterns were collected over a 2θ range of 15° to 80°, with a step size of 0.0262° holding for 0.4 s for each step. Additionally, LSF1:LiF–NaF–CaF2 (post-100 cycles) was scanned using a high-temperature stage XRK900 since the spent sample was more prone to absorb moisture. The sample was ramped up to 200 °C in an N2 atmosphere to remove hydrates. Phase analysis was performed using HighScore software. We examined the surface morphologies of LSF1 and LSF1:LiF–NaF–CaF2 using a Hitachi SU8700 field-emission scanning electron microscope (FESEM) coupled with energy-dispersive X-ray spectroscopy (EDS).

2.3 TGA-DSC and thermal conductivity measurements

We determined melting/crystallization enthalpy and temperature by means of a differential scanning calorimeter (DSC with ±2% accuracy) coupled with a thermogravimetric analyzer (TGA, TA-Instrument, SDT Q650). The heat flow was calibrated using a sapphire reference with a known heat capacity. Prior to each experiment, cell constant calibration was verified using aluminum wire to obtain a calibration constant, which was then used to correct the measured heat of fusion. In each experiment, we placed 10–13 mg of YSZ (yttria-stabilized zirconia) as inert material and then 10–15 mg of the sample into a 110 μm platinum (Pt) pan. Inert material was necessary to prevent the salt from sticking to the Pt pan upon melting.52 For the composite materials containing NaF–CaF2, an additional ∼30 mg of YSZ was placed on top to diminish the thermal losses. To minimize potential inaccuracies caused by the deflection of heat from shiny Pt pans, we used an alumina lid on top, resulting in more consistent measurements. The experiments were conducted over a temperature range of 150 °C, determined based on the melting/solidification point of the salt used in the ROMS (e.g., 670–820 °C for SCFM2:NaF–CaF2). First, the samples were heated up to 180 °C to remove the absorbed moisture, and the weight at the end of this step was used as the initial weight. The samples were then cycled between the lower and upper temperature limits at a ramping rate of 10 °C min−1, with 15 min isothermal steps. Typically, the first two cycles were carried out in an Ar atmosphere at a total gas flow rate of 200 ml min−1, followed by alternating between 20% O2/80% Ar at the upper temperature and Ar at the lower temperature. For the experiments under reducing conditions, samples were first ramped up to 730 °C under Ar and then exposed to 20% H2/80% Ar until equilibrium was reached. After that, the samples were ramped down to 580 °C under Ar, followed by exposure to 20% O2/80% Ar. Details regarding TGA-DSC analysis and calculation of overall energy density are described in the ESI.

We measured the thermal conductivities of LSF1, LiF–NaF–CaF2, and the composite material LSF1:LiF–NaF–CaF2via the transient plane source technique using the Hot Disc sensor, which is a widely accepted approach for determining thermal properties of materials.57–59 Details regarding this method can be found in the ESI.

3. Results and discussion

3.1 Compatibility between perovskite oxides and eutectic salt mixtures

The compatibility between various metal oxides and eutectic salt mixtures was first evaluated using XRD. The formation of new phases other than the target oxide and salt phases would indicate a reaction between the oxides and the salts. This is undesirable as it degrades the energy capacity of the sample, as demonstrated by the measured melting enthalpies of SF:LiF–NaF and SBF:LiF–NaF, detailed in Table S2 (exact compositions of metal oxides can be found in Table 1). Overall, 12 out of 25 samples screened were compatible. The XRD patterns of the compatible samples were presented in Fig. 2 and 3 and the identified crystal phases for all the samples were summarized in Table 3. In general, the Ca- and Ba-based oxides were less likely to react with NaF, CaF2, and NaCl. However, when LiF or MgF2 were introduced in the salt mixtures, the B-site cation(s) of the perovskite oxides tended to form new oxide phases with the cations of fluoride salts. Additionally, cations of SBF and SF led to the formation of new fluorides by breaking the eutectic phase of the salt mixture. Some of the resulting fluoride phases, such as SrF2 or KCaF3, can be associated with their relatively higher stability compared to initial fluoride phases, as shown in Table S1 based on data from the Materials Project database.60 Although the relative stability of fluorides based on the Materials Project database offers a useful guide, it cannot explain all the formed phases, since it does not consider the potential favorability of competing mixed oxide phases; the benefits and limitations of this approach are further discussed in ESI.
image file: d5ta02329g-f2.tif
Fig. 2 XRD patterns of composite materials with Ca-based perovskites (a) SCFM1:NaF–CaF2, (b) SCFM2:NaF–CaF2 and (c) SCFM2:NaF–NaCl.

image file: d5ta02329g-f3.tif
Fig. 3 XRD patterns of composite materials with La-based perovskites (a) LSF1:LiF–NaF–CaF2, (b) LSF1:MgF2–NaF–CaF2, (c) LSF1:Li2CO3–Na2CO3, (d) LSF2:LiF–NaF–CaF2, (e) LSF3:LiF–NaF–CaF2, (f) LSCM7391:LiF–NaF–CaF2, (g) LSFCo:LiF–NaF–CaF2, (h) LSF1:Li2MoO4 and (i) LSF2:Li2MoO4.
Table 3 The summary of compatibility between salt mixtures and metal oxides Undesirable phases are highlighted in italic
Salt mixture Perovskite XRD phases Compatibility (yes/no)
a Trace amount of SrMoO4 was detected. b Minor unidentified peaks were present in the XRD pattern.
Li2CO3–Na2CO3 SBF Na2CO3 SrFeO2.6, SrCO3, Li1.05Fe0.95O2, Sr2Fe3O6, Na3FeO3 N
LSF1 La0.8Sr0.2FeO3, LiNaCO3 Y
LiF–NaF–CaF2 CAM CaF2, NaF, Ca2AlMnO5, Li2MnO3, CaO, LiAlO2, CaMn7O12 N
SF NaF, Sr0.88Ca0.08Na0.02Fe0.02F2, Li1.05Fe0.95O2, CaO, FeF3 N
SBF NaF, Sr0.88Ca0.08Na0.02Fe0.02F2, Li0.5Fe0.5O2, Ca0.5Sr0.5FeO2, LiFeO2, LiBaF3,Sr3Fe2O6 N
SCMCo1 NaF, CaF2, CaMnO3, Li2MnO3 N
SCMCo2 NaF, CaF2, CaMnO2.656, Li1.33Mn0.667O2 N
LSF1 La0.8Sr0.2FeO3, CaF2, NaF, LiF Y
LSF2 La0.7Sr0.3FeO3, CaF2, NaF, LiF Y
LSF3 LaFeO3, CaF2, NaF, LiF Y
LSCoM2 La0.7Sr0.3CoO3, CaF2, NaF, LiF Y
LSCoM1 NaF, Sr0.4La0.6CoO3, Sr0.5Ca0.5F2, LiCoO2 N
LSFCo La0.8Sr0.2Co0.6Fe0.4O3, CaF2, NaF, LiF Y
NaF–CaF2 SCFM1 Sr0.3Ca0.7MnO3, NaF, CaF2 Y
SCFM2 Sr0.2Ca0.8MnO3, NaF, CaF2 Y
MgF2–NaF–CaF2 SCFM1 CaF2, Sr0.5Ca0.5MnO3, NaF, Na0.15Ca0.85F1.85, CaFe2O4, Na0.457Fe0.67Mn0.33O2 N
LSF1 La0.6Sr0.4FeO2.997, CaF2, NaF Y
NaF–NaCl SCFM2 Sr0.3Ca0.7MnO3, NaF, NaCl Y
NaF-KF SCFM2 NaF, CaMnO3, KCaF3, K3NaFe2O8b N
CAM NaF, CaMnO2.97, Ca2MnO4, CaAl2O4, KCaF3, KAlO2 N
LiF–CaF2 SCFM1 CaF2, Li1.259Mn0.519Fe0.225O2 N
LiF–NaF SF SrFeO2.6, LiF, NaF, SrF2, LiFeO2, Sr3Fe2O7, FeF3, Fe3O4b N
SBF LiF, NaF, SrF2, Li0.5Fe0.5O, Fe2O3b N
Li2MoO4 LSF1 Li2MoO4, LaFeO3 Y
LSF2 Li2MoO4, La0.6Sr0.4FeO3, SrMoO4 Ya


On the other hand, La-based oxides were revealed to be more stable as they showed less tendency to react with salt mixtures in general. Our results suggested that increasing Sr in the A-site reduced the stability of the oxide structure. The higher stability of perovskite oxides with rare earth metals compared to alkaline earth metals was also supported by Jacobs et al.'s study through convex hull analysis.61 Thus, lower Sr in the A-site ensured a compatible composite structure with LiF–NaF–CaF2 and MgF2–NaF–CaF2. This phenomenon was observed for LSCM2 and LSCM1; the former formed a compatible composite material with LiF–NaF–CaF2 while the latter couldn't. A similar case that supports the high stability of La-based perovskite oxides was observed for Li2CO3–Na2CO3. The carbonate salt formed a compatible composite with a La-based material while a reaction with a Sr-based oxide occurred, causing incompatibility. Regarding the composites containing Li2MoO4, a minor peak of SrMoO4 was detected from a possible reaction between LSF2 and Li2MoO4, whereas there seemed to be better compatibility for LSF1: Li2MoO4.

In our previous high-throughput study, we showed that among the substituted SrFeO3−δ-based materials, SCFM2 achieved the highest thermochemical energy density.38 Due to the high redox activity of SCFM2, SCFM-based composites stored heat in both thermochemical and latent forms. On the other hand, LSF-based composites have shown better compatibility with various metal oxides and higher stability in the long term. Considering that many waste streams contain reducible gases such as H2 and CO, we extended the application of LSF-based composites for chemical energy recovery from the waste gas. Therefore, SCFM and LSF-containing composites were focused upon, with further details provided in Sections 3.2 and 3.3.

3.2 SCFM-based composite materials

3.2.1 Phase change properties and redox activity. Here, we assessed the latent heat and melting/solidification points of the composite materials under redox cycling conditions, the key parameters for thermal energy storage of molten salts.21,25 The significant results for SCFM-based composites are summarized in Table 4, with additional data in Table S2 and Fig. S3–S9. This evaluation was essential in confirming that phase change properties of composite materials align with those of the individual salts, thereby validating the compatibility between salt and perovskites. For example, SCFM2:NaF–NaCl exhibited a large discrepancy between the theoretical salt properties and measured properties of the composite, suggesting a potential reaction between salt and perovskite during redox cycling; further details are provided in the ESI. Meanwhile, the composite material SCFM2:NaF–CaF2 with a weight ratio of 0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6 has shown promising performance in terms of high latent heat of ∼532 kJ kgsalt−1 (mechanical stability information can be found in Section 5 of the ESI). The measured latent heat for the composite material was slightly lower than that of pure salt, as shown in Table 4. It should be noted that variations up to ±10% in repeated measurements were observed, likely due to differences in the Pt pan geometry and varied contact between the salt and the inert material at the bottom of the pan. Also, the melting point of the composite (798 °C) was measured to be slightly lower than that of pure salt (∼805 °C).
Table 4 Measured melting enthalpy (kJ kgsalt−1) and melting points (°C) of composite materials. The weight ratios of eutectic salt mixtures are provided inTable 2
Sample name (weight ratio) Melting enthalpy (kJ kgsalt−1) Melting temperature (°C)
Reported Measured (±10%) Reported Measured
NaF–CaF2 560–600 561.80 810 804.67
NaF–CaF2:SCFM2 (0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6) 560–600 532.47 810 797.91
NaF–NaCl:SCFM2 (0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5) 572 340.84 674 672.13


In addition, we examined the redox activity of the SCFM2:NaF–CaF2, associated with O2 release and uptake of the perovskite oxides during the reduction and oxidation steps, respectively. Upon switching from Ar to 20% O2/Ar, an oxidation capacity of 1.05 wt% per oxide was determined. This was slightly less than the redox capacity (1.13 wt%) of pure perovskite under the same conditions (Fig. S7), indicating that molten salt may slightly inhibit oxygen diffusion and exchange. When the atmosphere was returned to Ar, the reduction capacity matched the oxidation, indicating a reversible oxygen exchange behavior. Using the previously obtained enthalpy data of SCFM2, a thermochemical energy density of ∼105 kJ kgoxide−1 (∼42 kJ kgcomposite−1) was calculated. With the contributions from the sensible heat of salt and oxide, an overall energy density of ∼523 kJ kg−1 (4th cycle) was determined. Although the contribution of thermochemical energy was less than latent heat, using a redox-active support material instead of an inert material was advantageous for the overall energy density of the composite.

We evaluated the stability of phase change properties and redox activity in SCFM2:NaF–CaF2 (0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6). Under a temperature swing of 740–890 °C, the composite exhibited a weight loss of 3.92 wt% (5.88 wt% per salt) over 10 redox cycles, which can be attributed to the evaporation of fluoride salt due to high vapor pressures.52 However, the weight loss was still significantly lower than the loss of ∼10.2 wt% in the pure salt under similar conditions (Fig. S3), indicating that perovskite stabilizes the fluoride salt by inhibiting its evaporation. To further decrease this loss, the experiments were conducted under a swing between 670–820 °C, with a layer of YSZ particles covering the composite. As shown in Fig. S4–S6 and 4a, both the composite material and salt demonstrated more stable performance under this lower temperature range. Over 10 cycles, the latent heat decreased from ∼532 to ∼513 kJ kgsalt−1 in the composite. The redox capacity of SCFM2 also gradually declined from 1.05 to 0.56 wt% (per oxide) over the 10 cycles (Fig. 4b), possibly due to the partial decomposition of SCFM2 or the fluoride salt suppressing oxygen diffusion. Despite the slight deactivation, the overall energy density of the composite material remained high after 10 cycles (∼501 kJ kg−1).


image file: d5ta02329g-f4.tif
Fig. 4 TGA-DSC measurements for SCFM2:NaF–CaF2 with the weight ratio of 0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6 at 670 °C/20% O2–820 °C/Ar during 10 cycles. (a) Overall energy density (kJ kg−1), (b) weight change (%) normalized to the weight of SCFM2. Latent heat is the measured melting enthalpy from DSC. Thermochemical heat is calculated using the previous data on SCFM2.38Sensible heat is based on estimated heat capacities through an additive principle using NIST database.62
3.2.2 Long-term performance evaluation. Despite the slight deactivation of SCFM2:NaF–CaF2 over 10 cycles, its good redox activity and large latent heat capacity made it an interesting candidate for long-term performance evaluation. As shown in Fig. 5a and S8, the overall energy density decreased from ∼523 to ∼430 kJ kg−1 over 100 cycles under the conditions of 670 °C/20% O2–820 °C/Ar, with a 23% reduction in latent heat. This deactivation is likely due to the evaporation of the fluoride salt, as indicated by an 11.6 wt% loss, suggesting that SCFM2 was unable to fully stabilize the NaF–CaF2 salt material. Choosing a salt mixture with a lower melting point could potentially enhance the stability of ROMS composites by lowering the thermal losses.
image file: d5ta02329g-f5.tif
Fig. 5 TGA-DSC measurements for SCFM2:NaF–CaF2 with the weight ratio of 0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6 at 670 °C/20% O2–820 °C/Ar during 100 cycles. (a) Overall energy density (kJ kgcomposite−1), (b) weight change (%) normalized to the weight of SCFM2). Latent heat is the measured melting enthalpy from DSC. Thermochemical heat is calculated using the previous data on SCFM2.38Sensible heat is based on estimated heat capacities through additive principle using NIST database.62

On the other hand, SCFM2 maintained its redox activity, although the redox capacity gradually decreased from ∼1.05 wt% to ∼0.45 wt%, reducing thermochemical heat from ∼105 to ∼50 kJ kgoxide−1 (∼42 to ∼20 kJ kgcomposite−1) over 100 cycles. Post-experimental XRD (Fig. S33) showed that the reduced perovskite was transitioned to a Brownmillerite phase (Sr2Fe2O5) with additional minor peaks suggesting the partial decomposition of the oxide, which would explain the decrease in thermochemical heat. However, phase identification was challenging due to the presence of inert material that could not be fully separated from the sample. Nevertheless, the XRD results indicated that compatibility between salt and oxide was maintained after 100 redox cycles. Despite the deactivation of SCFM2:NaF–CaF2, these results support the hypothesis that molten salts and perovskite oxides can be compatible, storing heat via both phase change of the molten salt and redox reactions of the metal oxide.

3.3 LSF-based composite materials

3.3.1 Phase change properties and redox-activity. Most of the compatible composite materials included La-containing perovskites due to their stability in the presence of salt mixtures. In SCFM2:NaF–CaF2, the high melting point of the salt restricted the operating temperature to higher temperatures (>670 °C). Meanwhile, La-based perovskites paired with lower melting point salts enabled lower operating temperatures, reducing thermal losses. The summary of the measurements for LSF-based composites is presented in Table 5 below, with additional data in Fig. S10–S25 and Table S2.
Table 5 Measured melting enthalpy (kJ kgsalt−1) and melting points (°C) of composite materials. The weight ratios of eutectic salt mixtures are provided inTable 2
Sample name (weight ratio) Melting enthalpy (kJ kgsalt−1) Melting temperature (°C)
Reported Measured (error bar ±10%) Reported Reported
LiF–NaF–CaF2 640 622.93 615 609.69
LSF1:LiF–NaF–CaF2 (0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5) 640 542.73 615 603.36
LSF1:LiF–NaF–CaF2 (0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6) 640 579.74 615 606.66
LSF2:LiF–NaF–CaF2 (0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5) 640 544.00 615 600.06
LSF3:LiF–NaF–CaF2 (0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5) 640 466.54 615 600.88
LSCoM2:LiF–NaF–CaF2 (0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5) 640 549.55 615 605.17
LSFCo:LiF–NaF–CaF2 (0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5) 640 537.41 615 602.98
LSFCo:LiF–NaF–CaF2 (0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6) 640 595.05 615 606.73
Li2MoO4 280 281.49 705 693.40
LSF1:Li2MoO4 (0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5) 280 254.59 705 685.08
LSF2:Li2MoO4 (0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5) 280 252.46 705 687.55
LSF2:Li2MoO4 (0.6[thin space (1/6-em)]:[thin space (1/6-em)]0.4) 280 219.95 705 688.18


Our results revealed that the oxide[thin space (1/6-em)]:[thin space (1/6-em)]salt ratio has a significant impact on the phase change property of the composite materials. Fig. 6 demonstrates that melting enthalpy for LSF1:LiF–NaF–CaF2 decreases with increasing oxide content. While the melting enthalpy of pure LiF–NaF–CaF2 was measured as ∼623 kJ kgsalt−1, it dropped to ∼580 kJ kgsalt−1 when mixed with LSF1 at an oxide[thin space (1/6-em)]:[thin space (1/6-em)]salt ratio of 0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6. Similar trends were also observed for the composites of NaF–CaF2:SCFM2, LSFC:LiF–NaF–CaF2, and LSF2:Li2MoO4. Since the absence of chemical interaction between the salt and oxide phase was confirmed by XRD, the decrease in the latent heat with increasing salt content can be attributed to physical interactions. Previous research has also observed latent heat reduction in a porous supporting medium and linked this to the confinement of the phase change material.63–65 Additionally, melting temperatures also decreased with increasing oxide contents, consistent with the previous findings.27,64,66 The LSF-based composite materials with the other salts either faced stability issues or did not have a competitive energy density due to low latent heat, as briefly discussed in the ESI (for LSF1:Li2CO3–Na2CO3 and LSF1:LiF–NaF–MgF2).


image file: d5ta02329g-f6.tif
Fig. 6 Comparison of LSF1:LiF–NaF–CaF2 at various salt amounts. (a) Normalized heat flows (W gsalt−1) and (b) latent heats (kJ kgsalt−1)

In terms of redox activity, most of the La-based perovskites in the composite materials failed to exchange their lattice oxygen during the redox cycles due to: (i) the intrinsic stability of these perovskite oxides, and (ii) the additional mass transfer resistance due to the presence of the salt. While pure LSFCo showed a redox capacity of ∼0.08 wt%, no significant weight change was observed for LSFCo in the composite (Fig. S18). Noting that the temperature range was not high enough to activate the redox behavior of La-based perovskite. Previous studies have shown that La-based perovskite can achieve high reaction enthalpy and oxygen capacity at elevated temperatures.67,68 Among the LSF-based composites, only LSF2 exhibited a weight gain corresponding to oxidation (Fig. S13, S22 and S23). Increased Sr[thin space (1/6-em)]:[thin space (1/6-em)]La ratio was found to benefit the redox activity by lowering the reduction temperature but also increased the likelihood of chemical interactions with the salt. In LSF2:Li2MoO4, the redox capacity increased from ∼0.08 to ∼0.15 wt% per oxide with oxide content increasing from 50 to 60%. Optimizing the oxide microstructure can potentially decrease the mass transfer resistance but LSF-based composites require a more reducing environment (e.g. higher temperatures or reducing gases) in order to exhibit substantial redox capacity. This will be further discussed in a later section.

3.3.2 Long-term performance evaluation. Due to its high latent heat storage and compatibility, LSF1:LiF–NaF–CaF2 with the weight ratio of 0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6 was selected as a promising candidate for long-term performance evaluation (see Section 5 in ESI with respect to mechanical stability). As shown in Fig. 7, the composite demonstrated excellent stability over 100 cycles under the conditions of 510 °C/20% O2–660 °C/Ar, with no significant change in the latent heat. The good stability of this composite material can be attributed to its lower operating temperature range compared to that of SCFM2:NaF–CaF2. The addition of LiF to NaF–CaF2 lowers the melting point, thus allowing for a lower operating temperature range and preventing salt weight loss from evaporation. Since no O2 release/uptake was observed, there was no thermochemical energy contributed to the overall energy density. After 100 cycles, the total energy density, including latent and sensible heat, remained as high as ∼534 kJ kg−1.
image file: d5ta02329g-f7.tif
Fig. 7 TGA-DSC measurements for LSF1:LiF–NaF–CaF2 with the weight ratio of 0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6 at 510 °C/20% O2–660 °C/Ar during 100 cycles. (a) Overall energy density (kJ kg−1). Latent heat is the measured melting enthalpy from DSC. Sensible heat is based on estimated heat capacities through additive principle using NIST database.62

Additionally, we compared the XRD pattern of the LSF1:LiF–NaF–CaF2 before and after 100 cycles in Fig. 8a. The additional peak corresponds to the thin layer of YSZ, which covered the bottom of the pan during the experiment. No significant change in the phases of perovskite and salts was seen. This shows that no reactions between LSF and fluoride salt occurred during redox cycles, thus the ROMS composite maintained its compatibility and energy density during 100 cycles. According to Fig. 8b and c, the morphology of the composite material was also maintained after 100 cycles (EDX mappings can be found in Fig. S36).


image file: d5ta02329g-f8.tif
Fig. 8 Comparison of fresh and spent (after 100 cycles between 510 °C/20% O2–660 °C/Ar) LSF1:LiF–NaF–CaF2 (0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6). (a) XRD patterns and SEM images of (b) after sintering, which corresponds to the morphology of composite material after 1 cycle (c) after 100 cycles.
3.3.3 Thermal conductivity. For LSF1: LiF–NaF–CaF2 (0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6), we also measured thermal conductivity, a key factor in heat transfer efficiency.11,14Table 6 presents the measured thermal conductivities and compares them with other composite materials reported for thermal energy storage. Using the transient plane source principle, the thermal conductivity of LSF1: LiF–NaF–CaF2 (0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6) was found to be 2.51 W m−1 K−1, which falls within the range of measured thermal conductivities of individual components. While LSF1 showed relatively low thermal conductivity, consistent with the results of other metal oxides in the literature,69,70 the elevated thermal conductivity of fluoride salt led to a competitively high thermal conductivity for the composite material compared to some other reported composites. The high thermal conductivity of the ROMS composite enables rapid heat exchange, enhancing adaptability in various reactor designs.
Table 6 Comparison of thermal conductivities at room temperature
Material Thermal conductivity (W m−1 K−1) Measurement method
LSF1 0.76 Transient
LiF–NaF–CaF2 2.96 Transient
LSF1:LiF–NaF–CaF2 (0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6) 2.51 Transient
LiNO3–NaNO3–KNO3–Ca(NO3)2:calcium silicate11 1.18 Steady state
NaNO3: modified diatomite25 ∼0.28 Transient
Li2CO3–Na2CO3:MgO:carbon23 ∼3–5.25 Transient
Polyethylene glycol:diatomite: expanded graphite28 0.32–0.67 Transient


3.3.4 Alternative applications under a reducing gas environment. Despite the stable performance of LSF1:LiF–NaF–CaF2 composite, the limited redox performance of La-based perovskites decreases the overall energy density. To address this, we explored an alternative usage of ROMS composites. The exhaust gas emitted by electric arc furnaces or blast furnaces in the steel industry carries substantial waste heat, often rich in reducing agents like H2 and CO8,71,72 which holds valuable potential for thermochemical energy storage applications. Thus, we performed experiments under a reducing gas atmosphere for a composition with Li2MoO4 since previous research indicated Mo salts in the liquid phase improve oxygen diffusion.73 Although LSF2 exhibited better potential for redox activity than LSF1 under cyclic conditions between 20% O2–Ar, LSF2:Li2MoO4 was not tested due to the trace amount of SrMoO4 impurity detected in its XRD pattern (Fig. 3i). Therefore, LSF1:Li2MoO4 (0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5) was tested as a potential candidate, with the results presented in Fig. 9 and S26–S32.
image file: d5ta02329g-f9.tif
Fig. 9 Comparison of LSF1, Li2MoO4, and LSF1:Li2MoO4 with the weight ratio of 0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5 during long reduction. (a) Weight changes (%) at 730 °C/20% H2 and (b) heat flow (mW) at 580/20% O2.

LSF1:Li2MoO4 (0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5) achieved thermochemical energy storage capacity as high as 1813 kJ kg−1 after a sufficiently long reduction time (∼8 h) to reach equilibrium. However, in electric arc furnaces, tap-to-time per batch is typically much shorter, around 30–70 min8,72 When a shorter reduction time of 35 min applied, the composite material still achieved an excellent thermochemical energy storage capacity of ∼664 kJ kg−1. Comparing this to the oxidation enthalpies of LSF1(∼239 kJ kg−1) and Li2MoO4 (∼683 kJ kg−1) (Table 7), it appears that the redox activity of Li2MoO4 primarily enhanced the energy storage capacity of LSF1: Li2MoO4 rather than LSF1. Additionally, reduction kinetics, shown in Fig. 9, indicate that rapid weight loss in LSF1: Li2MoO4 was mainly attributable to the fast reduction kinetics of Li2MoO4. The fast kinetics resulted in a ROMS composition with improved thermochemical energy compared to pure LSF1. Including the estimated sensible heat and latent heat, the overall energy density for LSF1: Li2MoO4 (0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5) reached 875 kJ kg−1.

Table 7 Weight changes (%) and energy densities of LSF1, Li2MoO4, and LSF1:Li2MoO4 (0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5). Weight loss and weight gain correspond to the weight changes in the samples during gas switch to 20% H2 and 20% O2, respectively
Material Weight loss (wt%) Weight gain (wt%) Oxidation enthalpy (kJ kg−1) ±10% Overall energy density (kJ kg−1)
Li2MoO4 10.0 8.17 682.7 1051
LSF1 (short reduction) 2.10 2.49 238.9 319.4
LSF1 (long reduction) 8.90 8.85 1309 1389
LSF1:Li2MoO4 (short reduction) 6.37 6.39 664.1 874.7
LSF1:Li2MoO4 (long reduction) 11.5 11.5 1813 2024


While Li2MoO4 exhibited rapid weight loss, weight gain didn't match weight loss in Li2MoO4, potentially caused by slow oxidation kinetics as shown in Fig. S28. Meanwhile weight loss and gain were approximately the same in LSF1 and LSF1: Li2MoO4, indicating reversible redox behaviors. This indicates that mixing LSF1 and Li2MoO4 created a synergistic benefit: LSF1 facilitates rapid oxidation and Li2MoO4 drives fast reduction. As can be seen from Fig. S31 and S32, in a cyclic experiment, the fast reduction and oxidation behavior of LSF1:Li2MoO4 with the weight ratio of 0.6[thin space (1/6-em)]:[thin space (1/6-em)]0.4 was maintained. While a detailed understanding of the reduction and oxidation mechanisms for this interesting composite is beyond the scope of this study, its promising performance can encourage future research aimed at recovering waste heat.

4. Comparison of ROMS composites

As can be seen from Table 8, ROMS composites offer superior thermal energy storage performance compared to phase change composites with inert skeletons. They can achieve higher energy densities within narrower temperature ranges. Fig. 10 compares the thermal energy densities of three ROMS composite materials with different performance features. LSF1:LiF–NaF–CaF2 exhibited the highest latent heat capacity of 580 kJ kgsalt−1 though it showed no redox activity under a pressure swing between 20% O2–Ar, leading to a total energy density of ∼530 kJ kgcomposite−1 over a relatively low-temperature range (510–660 °C). Meanwhile, SCFM2:NaF–CaF2 exhibited both thermochemical and latent heat based energy storage. Still, latent heat storage was the main contributor to its overall energy density of ∼523 kJ kg−1 under the cycling conditions of 670/20% O2–820 °C/Ar. Lastly, LSF1:Li2MoO4 achieved the highest overall energy density up to 875 kJ kg−1 at 580/20% O2–730 °C/20% H2, driven primarily by redox activity of both salt and oxide. This material is proposed for harnessing fuel containing off-gas from the steel industry. In terms of sensible heat storage, LiF–NaF–CaF2 had the highest capacity among salts, reaching 250 kJ kgsalt−1, while SCFM2 was expected to achieve the highest among oxides, at ∼125 kJ kgoxide−1. LSF1:LiF–NaF–CaF2 showed excellent stability and robustness over 100 cycles, whereas SCFM2:NaF–CaF2 showed deactivation with a gradual decline in latent and thermochemical heat over time. LSF1: Li2MoO4 showed good stability over the 5 cycles tested under a more reducing atmosphere.
Table 8 Comparison of energy densities storage densities over the corresponding temperature ranges
Material Energy storage density (kJ kg−1) Temperature range (°C)
SCFM2:NaF–CaF2 523 670–820
LSF1:LiF–NaF–CaF2 530 510–660
LSF1:Li2MoO4 875 580–730
NaNO3: Modified diatomite25 383 130–330
NaNO3:Ca(OH)2[thin space (1/6-em)]74 265–468 140–340
Graphite:Na2CO3–Li2CO3: MgO27 525 300–600
NaCl–KCl:diatomite10 393 550–750



image file: d5ta02329g-f10.tif
Fig. 10 Comparison of energy densities for SCFM2:NaF–CaF2 (0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6), LSF1:LiF–NaF–CaF2 (0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6), and LSF1: Li2MoO4 (0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5) under the redox cycling conditions of 670/20% O2–820 °C/Ar, 510/20% O2–660 °C/Ar, and 580/20% O2-730 °C/20% H2, respectively. The units of kJ kgcomposite−1were used for each component. Sensible heat is based on estimated heat capacities through additive principle using NIST database.62

5. Conclusions

This study introduces redox-active oxide-molten salt (ROMS) composites, where a porous perovskite oxide serves as a support to prevent salt leakage. This novel family of materials has the potential to utilize both latent heat from the phase transition of salt and thermochemical heat from the redox reactions to achieve high energy density within narrow temperature swings. Among 25 tested perovskite–salt combinations, 12 were found to be compatible with La-based perovskites showing superior compatibility and Sr and/or Ca-containing oxides exhibiting good redox activity. SCFM6271:NaF–CaF2 (0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6) was identified for both phase transition and redox-based energy storage with an overall capacity of ∼523 kJ kg−1 (670–820 °C) but faced stability and deactivation issues over the long term. Meanwhile, LSF1:NaF–CaF2–LiF (0.4[thin space (1/6-em)]:[thin space (1/6-em)]0.6) maintained a latent heat-based energy storage capacity of ∼530 kJ kg−1 although it did not exhibit redox activity under the cycling conditions of 510/20% O2–660 °C/Ar. It demonstrated excellent stability over 100 cycles, while compatibility and morphology were also maintained. The thermal conductivity of LSF1: LiF–NaF–CaF2 was found to be 2.51 W m−1 K−1. Lastly, LSF1: Li2MoO4 (0.5[thin space (1/6-em)]:[thin space (1/6-em)]0.5) exhibited high redox activity with an overall energy density up to ∼875 kJ kg−1 and was proposed as a promising candidate for recovering waste gas streams rich in residue fuels. The interesting characteristics and versatility of the ROMS composites reported in this study can potentially find applications for various thermal energy storage scenarios.

Data availability

Data supporting this article have been included as part of the ESI.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

This work was supported by the National Science Foundation (Grant No. CBET-2329857 and CBET-1923468). J. L. and S. R. were supported by the funding award from National Science Foundation (CBET-1943813). This work was performed in part at the Analytical Instrumentation Facility (AIF) at North Carolina State University, which is supported by the State of North Carolina and the National Science Foundation (award number ECCS-2025064). The AIF is a member of the North Carolina Research Triangle Nanotechnology Network (RTNN), a site in the National Nanotechnology Coordinated Infrastructure (NNCI).

References

  1. Fossil Fuels, https://www.eesi.org/topics/fossil-fuels/description#:%7E:text=Fossil%20fuels%E2%80%94including%20coal%2C%20oil,percent%20of%20the%20world's%20energy, accessed 2024-03-08 Search PubMed.
  2. Fossil fuels account for the largest share of U.S. energy production and consumption, https://www.eia.gov/todayinenergy/detail.php?id=45096, accessed 2024-03-08 Search PubMed.
  3. Greenhouse gas emissions, https://ourworldindata.org/greenhouse-gas-emissions, accessed 2024-03-08 Search PubMed.
  4. C. Forman, I. K. Muritala, R. Pardemann and B. Meyer, Estimating the Global Waste Heat Potential, Renewable Sustainable Energy Rev., 2016, 57, 1568–1579,  DOI:10.1016/j.rser.2015.12.192.
  5. M. Ja’fari, M. I. Khan, S. G. Al-Ghamdi, A. J. Jaworski and F. Asfand, Waste Heat Recovery in Iron and Steel Industry Using Organic Rankine Cycles, Chem. Eng. J., 2023, 477, 146925,  DOI:10.1016/j.cej.2023.146925.
  6. L. Miró, J. Gasia and L. F. Cabeza, Thermal Energy Storage (TES) for Industrial Waste Heat (IWH) Recovery: A Review, Appl. Energy, 2016, 179, 284–301,  DOI:10.1016/j.apenergy.2016.06.147.
  7. A. Vannoni, A. Sorce, A. Traverso and A. Fausto Massardo, Techno-Economic Optimization of High-Temperature Heat Pumps for Waste Heat Recovery, Energy Convers. Manage., 2023, 290, 117194,  DOI:10.1016/j.enconman.2023.117194.
  8. I. Alshehhi, W. Alnahdi, M. Ali, A. Bouabid and A. Sleptchenko, Assessment of Waste Heat Recovery in the Steel Industry, J. Sustain. Dev. Energy Water Environ. Syst., 2023, 11(2), 1–22,  DOI:10.13044/j.sdewes.d10.0440.
  9. F. Dal Magro, M. Jimenez-Arreola and A. Romagnoli, Improving Energy Recovery Efficiency by Retrofitting a PCM-Based Technology to an ORC System Operating under Thermal Power Fluctuations, Appl. Energy, 2017, 208, 972–985,  DOI:10.1016/j.apenergy.2017.09.054.
  10. G. Leng, G. Qiao, Z. Jiang, G. Xu, Y. Qin, C. Chang and Y. Ding, Micro Encapsulated & Form-Stable Phase Change Materials for High Temperature Thermal Energy Storage, Appl. Energy, 2018, 217, 212–220,  DOI:10.1016/j.apenergy.2018.02.064.
  11. Z. Jiang, G. Leng, F. Ye, Z. Ge, C. Liu, L. Wang, Y. Huang and Y. Ding, Form-Stable LiNO3 –NaNO3–KNO3–Ca(NO3)2/Calcium Silicate Composite Phase Change Material (PCM) for Mid-Low Temperature Thermal Energy Storage, Energy Convers. Manage., 2015, 106, 165–172,  DOI:10.1016/j.enconman.2015.09.035.
  12. I. Sarbu and C. Sebarchievici, A Comprehensive Review of Thermal Energy Storage, Sustainability, 2018, 10(1), 191,  DOI:10.3390/su10010191.
  13. A. Caraballo, S. Galán-Casado, Á. Caballero and S. Serena, Molten Salts for Sensible Thermal Energy Storage: A Review and an Energy Performance Analysis, Energies, 2021, 14(4), 1197,  DOI:10.3390/en14041197.
  14. T. Wang, D. Mantha and R. G. Reddy, Novel High Thermal Stability LiF–Na2CO3–K2CO3 Eutectic Ternary System for Thermal Energy Storage Applications, Sol. Energy Mater. Sol. Cells, 2015, 140, 366–375,  DOI:10.1016/j.solmat.2015.04.033.
  15. R. Roper, M. Harkema, P. Sabharwall, C. Riddle, B. Chisholm, B. Day and P. Marotta, Molten Salt for Advanced Energy Applications: A Review, Ann. Nucl. Energy, 2022, 169, 108924,  DOI:10.1016/j.anucene.2021.108924.
  16. T. Wang, D. Mantha and R. G. Reddy, Thermal Stability of the Eutectic Composition in LiNO3–NaNO3–KNO3 Ternary System Used for Thermal Energy Storage, Sol. Energy Mater. Sol. Cells, 2012, 100, 162–168,  DOI:10.1016/j.solmat.2012.01.009.
  17. R. W. Bradshaw and N. P. Siegel, Molten Nitrate Salt Development for Thermal Energy Storage in Parabolic Trough Solar Power Systems, in ES2008, ASME 2008 2nd International Conference on Energy Sustainability, 2008, vol. 2, pp. 631–637,  DOI:10.1115/ES2008-54174.
  18. T. Wang, D. Mantha and R. G. Reddy, Novel Low Melting Point Quaternary Eutectic System for Solar Thermal Energy Storage, Appl. Energy, 2013, 102, 1422–1429,  DOI:10.1016/j.apenergy.2012.09.001.
  19. J. Sunku Prasad, P. Muthukumar, F. Desai, D. N. Basu and M. M. Rahman, A Critical Review of High-Temperature Reversible Thermochemical Energy Storage Systems, Appl. Energy, 2019, 254, 113733,  DOI:10.1016/j.apenergy.2019.113733.
  20. A. Awad, A. Burns, M. Waleed, M. Al-Yasiri and D. Wen, Latent and Sensible Energy Storage Enhancement of Nano-Nitrate Molten Salt, Sol. Energy, 2018, 172, 191–197,  DOI:10.1016/j.solener.2018.04.012.
  21. M. M. Kenisarin, High-Temperature Phase Change Materials for Thermal Energy Storage, Renewable Sustainable Energy Rev., 2010, 14(3), 955–970,  DOI:10.1016/j.rser.2009.11.011.
  22. E. González-Roubaud, D. Pérez-Osorio and C. Prieto, Review of Commercial Thermal Energy Storage in Concentrated Solar Power Plants: Steam vs. Molten Salts, Renewable Sustainable Energy Rev., 2017, 80, 133–148,  DOI:10.1016/j.rser.2017.05.084.
  23. Z. Ge, F. Ye, H. Cao, G. Leng, Y. Qin and Y. Ding, Carbonate-Salt-Based Composite Materials for Medium- and High-Temperature Thermal Energy Storage, Particuology, 2014, 15, 77–81,  DOI:10.1016/j.partic.2013.09.002.
  24. T. Qian, J. Li, X. Min, Y. Deng, W. Guan and L. Ning, Diatomite: A Promising Natural Candidate as Carrier Material for Low, Middle and High Temperature Phase Change Material, Energy Convers. Manage., 2015, 98, 34–45,  DOI:10.1016/j.enconman.2015.03.071.
  25. F. Jiang, Z. Ge, X. Ling, D. Cang, L. Zhang and Y. Ding, Improved Thermophysical Properties of Shape-Stabilized NaNO3 Using a Modified Diatomite-Based Porous Ceramic for Solar Thermal Energy Storage, Renewable Energy, 2021, 179, 327–338,  DOI:10.1016/j.renene.2021.07.023.
  26. R. Li, J. Zhu, W. Zhou, X. Cheng and Y. Li, Thermal Properties of Sodium Nitrate-Expanded Vermiculite Form-Stable Composite Phase Change Materials, Mater. Des., 2016, 104, 190–196,  DOI:10.1016/j.matdes.2016.05.039.
  27. Z. Ge, F. Ye and Y. Ding, Composite Materials for Thermal Energy Storage: Enhancing Performance through Microstructures, ChemSusChem, 2014, 7(5), 1318–1325,  DOI:10.1002/cssc.201300878.
  28. S. Karaman, A. Karaipekli, A. Sarı and A. Biçer, Polyethylene Glycol (PEG)/Diatomite Composite as a Novel Form-Stable Phase Change Material for Thermal Energy Storage, Sol. Energy Mater. Sol. Cells, 2011, 95(7), 1647–1653,  DOI:10.1016/j.solmat.2011.01.022.
  29. Y. Deng, J. Li, T. Qian, W. Guan and X. Wang, Preparation and Characterization of KNO3/Diatomite Shape-Stabilized Composite Phase Change Material for High Temperature Thermal Energy Storage, J. Mater. Sci. Technol., 2017, 33(2), 198–203,  DOI:10.1016/j.jmst.2016.02.011.
  30. L. Sang and Y. Xu, Form Stable Binary Chlorides/Expanded Graphite Composite Material with Enhanced Compressive Strength for High Temperature Thermal Storage, J. Energy Storage, 2020, 31, 101611,  DOI:10.1016/j.est.2020.101611.
  31. L. André, S. Abanades and G. Flamant, Screening of Thermochemical Systems Based on Solid-Gas Reversible Reactions for High Temperature Solar Thermal Energy Storage, Renewable Sustainable Energy Rev., 2016, 64, 703–715,  DOI:10.1016/j.rser.2016.06.043.
  32. T. Block and M. Schmücker, Metal Oxides for Thermochemical Energy Storage: A Comparison of Several Metal Oxide Systems, Sol. Energy, 2016, 126, 195–207,  DOI:10.1016/j.solener.2015.12.032.
  33. X. Han, L. Wang, H. Ling, Z. Ge, X. Lin, X. Dai and H. Chen, Critical Review of Thermochemical Energy Storage Systems Based on Cobalt, Manganese, and Copper Oxides, Renewable Sustainable Energy Rev., 2022, 158, 112076,  DOI:10.1016/j.rser.2022.112076.
  34. X. Chen, M. Kubota, S. Yamashita and H. Kita, Investigation of Sr-Based Perovskites for Redox-Type Thermochemical Energy Storage Media at Medium-High Temperature, J. Energy Storage, 2021, 38, 102501,  DOI:10.1016/j.est.2021.102501.
  35. N. Gokon, T. Yawata, S. Bellan, T. Kodama and H.-S. Cho, Thermochemical Behavior of Perovskite Oxides Based on LaxSr1-x(Mn, Fe, Co)O3-δ and BaySr1-yCoO3-δ Redox System for Thermochemical Energy Storage at High Temperatures, Energy, 2019, 171, 971–980,  DOI:10.1016/j.energy.2019.01.081.
  36. E. Mastronardo, X. Qian, J. M. Coronado and S. M. Haile, Impact of La Doping on the Thermochemical Heat Storage Properties of CaMnO3-δ, J. Energy Storage, 2021, 40, 102793,  DOI:10.1016/j.est.2021.102793.
  37. F. Jin, C. Xu, H. Yu, X. Xia, F. Ye, X. Li, X. Du and Y. Yang, CaCo0.05Mn0.95O3−δ: A Promising Perovskite Solid Solution for Solar Thermochemical Energy Storage, ACS Appl. Mater. Interfaces, 2021, 13(3), 3856–3866,  DOI:10.1021/acsami.0c18207.
  38. R. Cai, H. Bektas, X. Wang, K. McClintock, L. Teague, K. Yang and F. Li, Accelerated Perovskite Oxide Development for Thermochemical Energy Storage by a High-Throughput Combinatorial Approach, Adv. Energy Mater., 2023, 13(18), 2203833,  DOI:10.1002/aenm.202203833.
  39. B. Bulfin, J. Vieten, D. E. Starr, A. Azarpira, C. Zachäus, M. Hävecker, K. Skorupska, M. Schmücker, M. Roeb and C. Sattler, Redox Chemistry of CaMnO3 and Ca0.8Sr0.2MnO3 Oxygen Storage Perovskites, J. Mater. Chem. A, 2017, 5(17), 7912–7919,  10.1039/C7TA00822H.
  40. S. M. Babiniec, E. N. Coker, J. E. Miller and A. Ambrosini, Investigation of La Sr1−Co M1−O3− (M = Mn, Fe) Perovskite Materials as Thermochemical Energy Storage Media, Sol. Energy, 2015, 118, 451–459,  DOI:10.1016/j.solener.2015.05.040.
  41. E. Mastronardo, X. Qian, J. M. Coronado and S. M. Haile, The Favourable Thermodynamic Properties of Fe-Doped CaMnO 3 for Thermochemical Heat Storage, J. Mater. Chem. A, 2020, 8(17), 8503–8517,  10.1039/D0TA02031A.
  42. S. M. Babiniec, E. N. Coker, J. E. Miller and A. Ambrosini, Doped Calcium Manganites for Advanced High-Temperature Thermochemical Energy Storage, Int. J. Energy Res., 2016, 40(2), 280–284,  DOI:10.1002/er.3467.
  43. D. Yilmaz, E. Darwish and H. Leion, Utilization of Promising Calcium Manganite Oxygen Carriers for Potential Thermochemical Energy Storage Application, Ind. Eng. Chem. Res., 2021, 60(3), 1250–1258,  DOI:10.1021/acs.iecr.0c05182.
  44. L. Imponenti, K. J. Albrecht, R. J. Braun and G. S. Jackson, Measuring Thermochemical Energy Storage Capacity with Redox Cycles of Doped-CaMnO 3, ECS Trans., 2016, 72(7), 11–22,  DOI:10.1149/07207.0011ecst.
  45. L. Imponenti, K. J. Albrecht, J. W. Wands, M. D. Sanders and G. S. Jackson, Thermochemical Energy Storage in Strontium-Doped Calcium Manganites for Concentrating Solar Power Applications, Sol. Energy, 2017, 151, 1–13,  DOI:10.1016/j.solener.2017.05.010.
  46. E. Darwish, M. Mansouri, D. Yilmaz and H. Leion, Effect of Mn and Cu Substitution on the SrFeO3 Perovskite for Potential Thermochemical Energy Storage Applications, Processes, 2021, 9(10), 1817,  DOI:10.3390/pr9101817.
  47. E. J. Popczun, D. N. Tafen, S. Natesakhawat, C. M. Marin, T.-D. Nguyen-Phan, Y. Zhou, D. Alfonso and J. W. Lekse, Temperature Tunability in Sr1−xCaxFeO3−δ for Reversible Oxygen Storage: A Computational and Experimental Study, J. Mater. Chem. A, 2020, 8(5), 2602–2612,  10.1039/C9TA09307A.
  48. F. Li, R. Cai, L. M. Neal and K. H. Bektas, Oxide-Molten Salt Composites for High-Performance Thermal Energy Storage, US Pat., US20240299911A1, 2024 Search PubMed.
  49. H. Bektas, R. Cai, L. Brody and F. Li, Structural and Thermodynamic Assessment of Ba and Ba/Mg Substituted SrFeO3−δ for “Low-Temperature” Chemical Looping Air Separation, Energy Fuels, 2024, 38(12), 11107–11118,  DOI:10.1021/acs.energyfuels.4c00859.
  50. L. Marianowski and H. Maru, Latent Heat Thermal Energy Storaap Systems above 450 C, in 12th Intersociety Energy Conversion Engineering Conference, 1977, vol. 1, pp. 555–566 Search PubMed.
  51. W. Phillips and J. Stearns, Advanced Latent Heat of Fusion Thermal Energy Storage for Solar Power Systems, in 20th Intersociety Energy Conversion Engineering Conference, 1985, vol. 2, pp. 2.384–2.391 Search PubMed.
  52. A. K. Misra, Fluoride Salts as Phase Change Materials for Thermal Energy Storage in the Temperature Range 1000–1400 K: Thermal Analysis and Heat of Fusion Measurements, J. Electrochem. Soc., 1988, 135(4), 850–854,  DOI:10.1149/1.2095808.
  53. J. D. Whittenberger and A. K. Misra, Identification of Salt—Alloy Combinations for Thermal Energy Storage Applications in Advanced Solar Dynamic Power Systems, J. Mater. Eng., 1987, 9(3), 293–302,  DOI:10.1007/BF02834148.
  54. N. Verdiev, E. Iskenderov, P. Arbukhanova and A. Amadziev, ТРЕХКОМПОНЕНТНАЯ СИСТЕМА Na//F, Cl,Br (English Translation:Three-component system Na/F, Cl, Br. Izvestiya VUZov. Severo-Kavkazskii Region), Nat. Sci., 2006, 56–61 Search PubMed.
  55. C. W. Bale, E. Bélisle, P. Chartrand, S. A. Decterov, G. Eriksson, A. E. Gheribi, K. Hack, I.-H. Jung, Y.-B. Kang, J. Melançon, A. D. Pelton, S. Petersen, C. Robelin, J. Sangster, P. Spencer and M.-A. V. Ende, FactSage Thermochemical Software and Databases, 2010–2016, Calphad, 2016, 54, 35–53,  DOI:10.1016/j.calphad.2016.05.002.
  56. E. Takayama-Muromachi, A. Navrotsky and S. Yamaoka, Calorimetric Study of High-Pressure Polymorphs of Li2WO4 and Li2MoO4, J. Solid State Chem., 1986, 65(2), 241–250,  DOI:10.1016/0022-4596(86)90059-9.
  57. S. E. Gustafsson, Transient Plane Source Techniques for Thermal Conductivity and Thermal Diffusivity Measurements of Solid Materials, Rev. Sci. Instrum., 1991, 62(3), 797–804,  DOI:10.1063/1.1142087.
  58. M. Gustavsson, E. Karawacki and S. E. Gustafsson, Thermal Conductivity, Thermal Diffusivity, and Specific Heat of Thin Samples from Transient Measurements with Hot Disk Sensors, Rev. Sci. Instrum., 1994, 65(12), 3856–3859,  DOI:10.1063/1.1145178.
  59. Y. He, Rapid Thermal Conductivity Measurement with a Hot Disk Sensor, Thermochim. Acta, 2005, 436(1–2), 122–129,  DOI:10.1016/j.tca.2005.06.026.
  60. A. Jain, S. P. Ong, G. Hautier, W. Chen, W. D. Richards, S. Dacek, S. Cholia, D. Gunter, D. Skinner, G. Ceder and K. A. Persson, Commentary: The Materials Project: A Materials Genome Approach to Accelerating Materials Innovation, APL Mater., 2013, 1(1), 011002,  DOI:10.1063/1.4812323.
  61. R. Jacobs, T. Mayeshiba, J. Booske and D. Morgan, Material Discovery and Design Principles for Stable, High Activity Perovskite Cathodes for Solid Oxide Fuel Cells, Adv. Energy Mater., 2018, 8(11), 1702708,  DOI:10.1002/aenm.201702708.
  62. M. Chase Jr. NIST-JANAF Themochemical Tables, American Chemical Society, Washington DC, 4th edn, 1998, vol. 9 Search PubMed.
  63. J. Lopez, G. Caceres, E. Palomo Del Barrio and W. Jomaa, Confined Melting in Deformable Porous Media: A First Attempt to Explain the Graphite/Salt Composites Behaviour, Int. J. Heat Mass Transfer, 2010, 53(5–6), 1195–1207,  DOI:10.1016/j.ijheatmasstransfer.2009.10.025.
  64. A. Anagnostopoulos, M. E. Navarro, M. Stefanidou, Y. Ding and G. Gaidajis, Red Mud-Molten Salt Composites for Medium-High Temperature Thermal Energy Storage and Waste Heat Recovery Applications, J. Hazard. Mater., 2021, 413, 125407,  DOI:10.1016/j.jhazmat.2021.125407.
  65. R.-A. Mitran, D. Lincu, L. Buhǎlţeanu, D. Berger and C. Matei, Shape-Stabilized Phase Change Materials Using Molten NaNO3 – KNO3 Eutectic and Mesoporous Silica Matrices, Sol. Energy Mater. Sol. Cells, 2020, 215, 110644,  DOI:10.1016/j.solmat.2020.110644.
  66. Q. Guo and T. Wang, Study on Preparation and Thermal Properties of Sodium Nitrate/Silica Composite as Shape-Stabilized Phase Change Material, Thermochim. Acta, 2015, 613, 66–70,  DOI:10.1016/j.tca.2015.05.023.
  67. E. Mastronardo, X. Qian, J. M. Coronado and S. M. Haile, Impact of La Doping on the Thermochemical Heat Storage Properties of CaMnO3-δ, J. Energy Storage, 2021, 40, 102793,  DOI:10.1016/j.est.2021.102793.
  68. H. E. Bush, R. Datta and P. G. Loutzenhiser, Aluminum-Doped Strontium Ferrites for a Two-Step Solar Thermochemical Air Separation Cycle: Thermodynamic Characterization and Cycle Analysis, Sol. Energy, 2019, 188, 775–786,  DOI:10.1016/j.solener.2019.06.059.
  69. W. Pan, S. R. Phillpot, C. Wan, A. Chernatynskiy and Z. Qu, Low Thermal Conductivity Oxides, MRS Bull., 2012, 37(10), 917–922,  DOI:10.1557/mrs.2012.234.
  70. Y. Liu, K. Chu, Y. Zhou, Y. Li, W. Li and B. Liu, Discovery of Orthorhombic Perovskite Oxides with Low Thermal Conductivity by First-Principles Calculations, J. Adv. Ceram., 2022, 11(10), 1596–1603,  DOI:10.1007/s40145-022-0632-0.
  71. K. Takahashi, T. Nouchi, M. Sato and T. Ariyama, Perspective on Progressive Development of Oxygen Blast Furnace for Energy Saving, ISIJ Int., 2015, 55(9), 1866–1875,  DOI:10.2355/isijinternational.ISIJINT-2015-196.
  72. M. Kirschen, H. Pfeifer, F. J. Wahlers and H. Mees, Off-Gas Measurements for Mass and Energy Balances of Stainless Steel EAF, in Electric Furnace Conference, 2001, vol. 59, pp. 737–748 Search PubMed.
  73. S. Yusuf, L. Neal, Z. Bao, Z. Wu and F. Li, Effects of Sodium and Tungsten Promoters on Mg6MnO8-Based Core–Shell Redox Catalysts for Chemical Looping—Oxidative Dehydrogenation of Ethane, ACS Catal., 2019, 9(4), 3174–3186,  DOI:10.1021/acscatal.9b00164.
  74. Q. Yu, Z. Jiang, L. Cong, T. Lu, B. Suleiman, G. Leng, Z. Wu, Y. Ding and Y. Li, A Novel Low-Temperature Fabrication Approach of Composite Phase Change Materials for High Temperature Thermal Energy Storage, Appl. Energy, 2019, 237, 367–377,  DOI:10.1016/j.apenergy.2018.12.072.

Footnotes

Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d5ta02329g
Present address: School of Mechanical Engineering, Shanghai Jiao Tong University, 800 Dongchuan RD, Minhang District, Shanghai, China.

This journal is © The Royal Society of Chemistry 2025
Click here to see how this site uses Cookies. View our privacy policy here.