Printing of tin perovskite solar cells via controlled crystallization

Xuan Li ae, Giuseppe Nasti bc, Chris Dreessen d, Janardan Dagar e, Rico Meitzner e, Davide Amoroso c, Pier Luca Maffettone c, Thomas Kirchartz df, Eva Unger e, Antonio Abate *ce and Stoichko D. Dimitrov *a
aDepartment of Chemistry, School of Physical and Chemical Sciences, Queen Mary University of London, London, E1 4NS, UK. E-mail: s.dimitrov@qmul.ac.uk
bENEA Research Center Portici, Piazzale Enrico Fermi 1, Portici, 80055, Italy
cDepartment of Chemical, Materials and Production Engineering, University of Naples Federico II, Piazzale Tecchio 80, Fuorigrotta, Naples, 80125, Italy. E-mail: antonio.abate@helmholtz-berlin.de
dIEK5-Photovoltaik, Forschungszentrum Jülich, Jülich, 52425, Germany
eHelmholtz-Zentrum Berlin für Materialien und Energie GmbH, Hahn-Meitner-Platz 1, Berlin, 14109, Germany
fFaculty of Engineering and CENIDE, University of Duisburg-Essen, Carl-Benz-Str. 199, Duisburg, 47057, Germany

Received 24th September 2024 , Accepted 26th February 2025

First published on 5th March 2025


Abstract

The urgent need for sustainable electricity has driven progress in solar technologies, with perovskite photovoltaics standing out as a top contender. However, the presence of toxic lead in current perovskite devices necessitates the exploration of alternative materials. This study addresses the challenges associated with tin perovskite fabrication and the industrial scale-up of this lead-free technology. It introduces a new approach to regulate the key process of crystallization, involving a combination of new additives and a gas pulse to trigger and subsequently control nucleation and crystal growth. In situ optical spectroscopy probed the crystallization and enabled the optimization of the printing conditions. Solar cells were fabricated with a power conversion efficiency of 5.38% for 0.1 cm2, 4.02% for 1 cm2 and 2.31% for 5 cm2 devices. They were tested under indoor lighting conditions and functioned at similar efficiency levels, thereby demonstrating the potential of this technology for commercial applications. Our new crystallization control method for printing Sn perovskites enabled the fabrication of the first Sn-based solar cell via slot-die coating, which is ideally suited for roll-to-roll manufacturing. This innovation opens new avenues for the development of fully printed lead-free perovskite photovoltaics, contributing significantly to the advancement of sustainable energy technologies.


Introduction

Metal-halide organic–inorganic perovskite solar cells have become the most popular emerging solar cell technology because of their potential to expand the number of applications for solar cells, enabling simpler manufacturing and increasing the efficiency of silicon devices. However, there are bottlenecks for their commercialization due to environmental concerns and health issues related to the presence of soluble Pb in the structure.1 Sn is considered the most promising substitute for Pb in the perovskite crystal structure, as it offers similar electronic properties but potentially a lower toxicity and a smaller environmental impact.2 Furthermore, Sn perovskites and specifically the popular formamidinium Sn iodide (FASI) have a smaller bandgap (1.3 eV) and can reach 33% power conversion efficiency (PCE), which is higher than Pb-perovskite (31%) according to the Shockley–Queisser limit.3 The highest efficiency achieved thus far for Sn-based perovskite solar cells is 16.05%,4 compared to 26.7% for single-band gap Pb-based perovskite devices and 34.6%5,6 for Pb perovskite/silicon tandem monolithic devices.

Sn-perovskite films have mostly been deposited via spin coating, which is a solution deposition technique used in conjunction with an antisolvent treatment and a heating step to fully convert the wet thin film into a perovskite semiconductor. A key feature of the fabrication process is that Sn perovskite crystallization is ultrafast, which is due to the greater Lewis acidity of Sn2+ compared to Pb2+, leading to uncontrollable film nonuniformities.7 Slowing down crystallization has been key to achieving a broader processing window and better-quality films.7–9 One way to make this possible has been solvent engineering.9–11 For example, Nasti et al. reported 4-(tert-butyl) pyridine (tBP) as a host solvent replacing the oxidative dimethyl sulfoxide (DMSO) to form a stable intermediate state that retards crystallization.12 Another popular approach is based on using additives as regulators of the crystallization dynamics, such as Sn halides.9 Both, SnCl2 (ref. 13) and SnF2 (ref. 14–16) form a Sn-rich environment that compensates for Sn vacancy defects and minimizes the oxidation of Sn2+, thus achieving efficient devices. Due to the size difference between Cl and I, the Cl ion is pushed to the surface of the perovskite crystallites during crystallisation also causing a Sn-rich environment, while favourably changing the energy level alignment and improving charge collection17 by directing the growth of larger grains for better film coverage.18 Despite the advances in controlling crystallisation, the reports on printed Sn perovskites has been scare.19,20 This is unlike Pb perovskite solar cells which have been printed with PCE reaching over 20%.21–25

LaMer theory is the most used model to describe the nucleation and growth of crystalline materials from solution.26 According to this theory, after coating, the wet perovskite film undergoes four phases, as depicted in Fig. 1a. Initially, the solute concentration is lower than the saturation limit and the solution is in its stable phase. Over time, an increasing amount of solvent is removed from the thin film by evaporation or extraction, and the concentration of the solution overcomes the saturation threshold. In this metastable phase, the solutes can thermodynamically form nuclei, but the film remains liquid, as it is kinetically stable. If the concentration of the solution is allowed to increase further, the thin film undergoes spontaneous burst nucleation. As the number of nuclei increases the concentration of the thin film decreases leading to the fourth phase of crystal growth. This general picture can be slightly modified to consider the kinetics of the process. If the rate of solvent evaporation increases during the first two phases, the slope of the curve increases, as shown in Fig. 1b. This can be achieved by changing external process parameters, such as higher substrate temperature or higher convective flux (i.e., spin coater rotation speed), or as mentioned above by solvent or additive engineering. Although the slope and shape of the curve change, the saturation threshold remains unaffected, as it is a thermodynamic parameter of the system; however, the minimum concentration for spontaneous nucleation increases.27 The effect of this change is two-fold: the number of nuclei formed is higher due to higher supersaturation; the decrease in the solution concentration is faster because of the larger number of crystallization centers. The overall effect on perovskite crystallization is that a faster evaporation rate leads to a larger number of small grains, which is considered a sub-optimal morphology for perovskite solar cells due to high grain borders and, therefore, defects. However, a slow rate of solvent evaporation leads to a small number of nuclei, which grow slowly and form undesirable isolated dendrite structures.28


image file: d4se01321b-f1.tif
Fig. 1 (a) Representation of La Mer theory of crystallization (precursor concentration vs. time) showing the four fundamental phases of crystallization: stable, metastable, nucleation burst, and growth; (b) pictorial representation of the grain morphology of perovskite films formed via three different crystallization modes: fast solvent evaporation, slow solvent evaporation, and triggered crystallization. SEM micrography of grain morphologies; (c) without and (d) with crystallization triggering investigated in this study.

In this work, we introduce a new antisolvent-free approach for Sn perovskite film crystallization that utilizes a short gas pulse as a nucleation trigger and new additives that optimize the metastable and nucleation burst rates, leading to high-quality perovskite film formation. This enabled us to fabricate the first Sn perovskite films printed successfully via an industrially scalable slot-die coating technique. High-quality films were printed on 25 mm × 75 mm and 50 × 50 mm substrates. In situ photoluminescence (PL) and transmission spectroscopy were used to probe the crystallization dynamics and enabled us to compare the additives and conditions to achieve compact and pinhole-free films via slot-die coating. The champion printed device has 5.38% PCE for 0.1 cm2 active area and 4.02% for 1 cm2 active area and uses the new perovskite additive MASnCl3. This is the first report of a slot die-coated Sn-perovskite solar cell, demonstrating that despite its ultrafast crystallization kinetics roll-to-roll production using this technology is entirely possible. To further explore its potential technological applications at scale, we also demonstrate the feasibility of using Sn-perovskite solar cells for indoor photovoltaics.

Slot-die coated films, optimising crystallization via in situ optical analysis

In the crystallization mechanism shown in Fig. 1a, the nucleation-growth process can be controlled using a triggering action during the metastable phase of the thin liquid film.29 For Pb-perovskites, the most common trigger is the dripping of an antisolvent, whereas for single step Sn perovskite coating this has been the only option. Here we tested a trigger based on a short pulse of inert gas instead of antisolvent on slot-die coated films on 25 mm × 75 mm glass substrates. The precursor solution was made of FAI and SnI2 dissolved in DMF[thin space (1/6-em)]:[thin space (1/6-em)]tBP 6[thin space (1/6-em)]:[thin space (1/6-em)]4 volume ratio. tBP was used as a complexing agent to slow down the dynamic of crystallisation via formation of intermediate phases.12 We observed that the brief blow of N2 successfully triggers perovskite nucleation (Fig. 1b) to produce a morphology consisting of compact and large grains (Fig. 1d), instead of the dendritic structures seen without the gas pulse trigger (Fig. 1c). Printed films appeared red after the gas pulse but after annealing on a hot plate at 140 °C converted to black. In Pb perovskites, the timing of the nucleation trigger is known to be crucial for achieving dense and uniform films with well-orientated and large grains.30 Here, too, the timing of the gas pulse had to be optimized, as otherwise films were found to eventually crystallize without the outside trigger and produce very poor morphologies unsuitable for device fabrication, as shown in Fig. S1.

Additives were introduced to the precursor solution to change the slope of the crystallization curve (Fig. 1b). Initially three additives were tested (2.5 mol% concentration): SnCl2, a popular additive for Sn perovskites;13 MACl, a popular additive for FAPbI3 systems because of its ability to induce intermediate phases;31 and SnF2. The Sn-perovskite films with the corresponding additives are denoted as FASI-SnCl2, FASI-MACl, and FASI-SnF2. It was observed from the in situ PL spectra in Fig. 2a that FASI-SnCl2 and FASI-MACl had drastically different crystallization kinetics. Aiming at an intermediate crystallization rate, a new additive MASnCl3 (2.5 mol% concentration) was then created by mixing equimolar amounts of MACl and SnCl2. MASnCl3 has been reported to have a perovskite structure.32,33 A solubility test was carried out for each additive by preparing 1M stock solutions in DMF, results shown in Fig. S2. SnCl2 dissolved in DMF, while MACl had a low solubility in either DMF or tBP. Since MASnCl3 dissolved fine, we suggest that MACl binds with SnCl2 to dissolve in the precursor solution by forming MASnCl3.


image file: d4se01321b-f2.tif
Fig. 2 (a) In situ PL measurements on slot-die coated films (contour plots with blue being the zero baseline and red being the maxima) printed with FASI-SnCl2, FASI-MACl, FASI-MASnCl3 and FASI-SnF2. For a better comparison, the intensities of each measurement were normalized to the maximum PL intensity detected during the entire experiment. No signal evolution was observed for FASI-MACl. The corresponding in situ (b) PL peak intensity and (c) peak position changes as a function of time; FASI-MACl was excluded because of a lack of signal. The results after thermal annealing include the following: (d) steady-state PL spectra and (e) X-ray diffraction.

With the trigger, uniform films were successfully printed. Without the air pulse trigger, the films with all additives eventually self-crystallized and produced poor morphologies that were unsuitable for device fabrication (Fig. S1). The final PL peak energies of the samples (Fig. 2d and Table S1) indicate the successful formation of high-quality FASnI3 films,34 except for FASI-MACl, which displayed a slightly higher bandgap PL, possibly owing to distorted structures or vacancies.

Immediately after the slot die coating, the wet film was placed onto the in situ setup (shown in Fig. S3), and after a short gas pulse was applied, PL and transmission were recorded for 120 s (the natural drying time at room temperature under N2 environment) with a 1 s interval time to probe the effect of the gas pulse on the crystallization kinetics. PL signals arise from emissive species formed in the film during crystallization, and the PL peak energy is a direct indicator of their bandgap, while a high PL intensity is linked to high-density and defect-free crystals.35–39Fig. 2a presents the PL spectra evolution for all four films before the final thermal annealing (140 °C on a hot plate). FASI-SnCl2, FASI-MASnCl3 and FASI-SnF2 each showed a well-defined PL peak in the range of 1.7–1.8 eV formed immediately after the application of the gas pulse trigger. We link the formation of this peak to the burst nucleation of FASnI3 perovskite nanocrystals triggered by the gas pulse, as depicted in Fig. 1a and b.30,40 From the color maps in Fig. 2a, it is evident that FASI-SnF2 exhibits the fastest nucleation and crystal growth, while FASI-MASnCl3 has the slowest evolving PL and hence slowest crystallization. FASI-MACl did not exhibit PL evolution until the sample was moved to the hot plate (when crystallization occurred), indicating that the gas pulse did not trigger nucleation in this sample. The in situ transmission data (shown in Fig. S4) is consistent with this observation and show only precursor absorption from FASI-MACl. Furthermore, both the PL intensity and energy of FASI-SnF2 and FASI-SnCl2 approach a plateau, as expected from the crystallization mechanism shown in Fig. 1, where the plateau occurs owing to a drop in solute supersaturation and termination of the nucleation process.41 These in situ results reveal that additives can be used to control the crystallization rates of gas-triggered films. They also reveal that under the studied conditions, a Sn2+-rich environment enables faster nucleation, consistent with previous studies of additives,33 while MA+ slows down this process likely due to the formation of a strong MA-SnI3-tBP adduct in addition to the FA-SnI3-tBP adducts.12,42

A closer look at the PL intensity and PL energy changes as a function of time in Fig. 2b–d reveals that there are two distinct nucleation events in FASI-SnCl2 and FASI-SnF2, and even in FASI-MASnCl3. The first stage is complete within 3 seconds of the gas pulse and driven purely by fast solvent evaporation forced by the gas blow, while the second stage continues for tens of seconds and can be linked to the more gradual evaporation at room temperature of the more volatile of the two solvents, DMF. The existence of the two nucleation stages shows that the slot-die coated wet film is close to the metastable phase (Fig. 1) right before the gas pulse application (which forces evaporation and some nucleation likely on the top surface of the film). Despite the presence of stable nuclei after the gas pulse, as evidenced by the presence of PL, the second nucleation stage starts only after approximately 10 seconds when there is a transition from the metastable to the nucleation burst phase. The second stage was controlled by the additive, where the rate of crystallization followed the order: SnF2 > SnCl2 > MASnCl3 > MACl. The faster crystallisation for FASI-MASnCl3 compared to FASI-MACl is likely due to MA+ binding in the MASnCl3 perovskite structure and minimising the effect from the MA-SnI3-tBP adducts formation.43 The final stage of crystallization occurs during thermal annealing when the leftover DMF and the higher-boiling-point tBP solvent are evaporated. FASI-SnCl2, FASI-SnF2 and FASI-MASnCl3 end up with a PL peak maximum in between 1.41 and 1.42, indicative of high quality FASnI3 films (Fig. 2d).34,44 The small peak shift for FASI-MASnCl3 could be due to Cl and MA+ incorporation in the FASnI3 crystal structure forming mixed perovskite. However, FASI-MACl's PL peak is at 1.52 eV, which can be explained by the incorporation of Cl in the crystal lattice.3,44

Structural characterization

X-ray diffraction (XRD) experiments were conducted to analyze the crystal structures of the four perovskite films (Fig. 2e and Table S2). Note that the samples had to be exposed to air for a short time (<5 min) during sample loading, inevitably leading to oxidation. For FASnI3 films with an orthorhombic (Amm2) crystal structure, two dominant peaks can be identified, which are located around 14.0° corresponding to the (100) crystal plane and 28.22° corresponding to the (200) crystal plane. All four films showed the above two peaks with some differences in full width at half maximum, intensity, and peak position, which originate from their different crystallization kinetics and compositions. For the FASI-SnCl2 films, double peaks at 12.75° and 12.94° were assigned to the SnI4 species,45 indicating Sn oxidation. The FASI-MACl films showed sharp peaks corresponding to the (100) and (200) planes and strong SnI4 peaks at 12.87° and 25.53°. The other two peaks at 26.13° could not be identified, while the low-intensity peak at 31.55° corresponded to the (122) plane of FASnI3,46 suggesting more disordered films for this sample. The XRD pattern of FASI-MASnCl3 has only two peaks corresponding to the (100) and (200) planes, indicating preferential perovskite crystallization with a better stability compared to FASI-SnCl2 and FASI-MACl. The small shift in diffraction peaks for FASI-MASnCl3 (similar to FASI-SnCl2) could be due to Cl incorporation in the crystal structure. For FASI-SnF2, the two main peaks showed lower intensities than for FASI-MASnCl3, with one extra peak at approximately 12.24°. The peak positions and the corresponding species are listed in Table S2. Similarly to XRD, SEM images (Fig. S5 on glass and Fig. S6 on PEDOT/ITO) indicated the presence of either point defects, undesirable particles, or poor grain boundaries on the surface of most samples, except for the best quality films of FASI-MASnCl3 and FASI-SnF2 deposited on PEDOT[thin space (1/6-em)]:[thin space (1/6-em)]PSS. From these data, it can be concluded that all samples produced predominantly FASnI3 with preferential crystallization with (100) planes parallel to the film surface.46 FASI-MASnCl3 had the cleanest diffraction pattern and surface quality without contaminants or defects, suggesting the highest quality of crystals and densely packed films for this sample,47,48 which agrees with the PL spectral intensities of the annealed films. It also highlights the importance of controlling the rate of crystallisation that neither too fast nor too slow nucleation is beneficial for growing high quality perovskite crystals for slot-die coated films.

Fabrication of slot-die coated devices

FASnI3 devices were fabricated by slot-die coating the Sn-perovskite films with the architecture: glass/ITO/PEDOT[thin space (1/6-em)]:[thin space (1/6-em)]PSS/FASnI3/C60/BCP/Ag. Fig. 3 presents the JV curves of the champion devices and the distribution of device parameters. FASI-MASnCl3 and FASI-SnF2 showed the best Jsc, corresponding well to their higher steady-state PL and compact grains, as shown in Fig. S6 in SEM. FASI-MACl showed a lower Jsc, which is partly due to the lower IPCE from 550 to 850 nm (Fig. S7). From IPCE, the bandgap of all devices could be determined as roughly 1.41 eV (Fig. S7), this is consistent with the bandgap derived from PL for SnCl2, MASnCl3 and SnF2. However, for FASI-MACl the bandgap derived from PL was 1.52 eV. This suggests an anti-Stokes shift of more than 100 meV. The spectral shape shift of the IPCE in FASI-MACl and to an extent in FASI-SnCl2 suggests that different photoactive species are formed. One possible explanation is that some MA/FASnCl3 was formed at the expense of FASnI3 or greater density of Sn vacancies are present in the films.34,44Voc followed the same trend as Jsc, while the fill factor remained similar between samples. From the JV data in Fig. 3, it appears that the best additive is MASnCl3 and the FASI-MASnCl3 device reaches η = 4.2%.
image file: d4se01321b-f3.tif
Fig. 3 Comparison of the performance of FASnI3 devices printed with the four additives studied, SnCl2, MACl, MASnCl3, SnF2. (a) JV scans; (b) light-intensity-dependent photoluminescence quantum yield of each sample (full device stack); (c) JV performance distribution (F for forward and R for reverse scans) of each sample.

To investigate recombination in the full device stacks, we measured the photoluminescence quantum yield (PLQY). The full spectra of the light-intensity-dependent steady-state photoluminescence are shown in Fig. S8. From Fig. 3b, it can be seen that the PLQY of each sample is independent of light intensity, which can be explained by the high doping density of Sn perovskites.49,50 For a doped semiconductor in low-level injection, all recombination mechanisms become linear in charge carrier concentration, so that the PLQY remains constant.51 Furthermore, the PLQY values are high in comparison to what is expected from the measured Voc values. This indicates an energetic mismatch in the device.52–54 In reverse, it follows that the quality of the printed Sn perovskites is higher than the low Voc values suggest. Comparing between additives, FASI-MASnCl3 shows the highest PLQY which is consistent with its better performance in devices and better film and crystal quality. Furthermore, the bulk is not primarily responsible for the Voc loss, which could be reduced by using an ETL with energy levels that better match the perovskite layer.55 Indeed, the PLQY is comparable to some high-performance Pb perovskite solar cells.56

The MASnCl3 molar concentration was optimized to further improve the performance. The results (Fig. S9) show that 7.5 mol% is the optimal molar concentration. We suggest that up to 7.5 mol%, MASnCl3 can be incorporated into the FASnI3 structure and form a mixed perovskite phase, which causes the small PL peak shift and broadening. It appears that a phase separation occurs between 7.5 mol% and 10 mol%, where due to energy level misalignment, the MASnCl3 phase starts to form a blocking layer and at 12.5 mol%, it becomes a blocking layer causing decreased shunt resistance hindering the extraction of charge carriers. Simultaneously, the series resistance, derived from the slope dV/dJ at Voc, increased as the additive concentration increased from 7.5 to 10%. If a new phase with a larger bandgap is formed, then the increase in Jsc with MASnCl3 is impressive, as it means that the mixed phase also has a better charge carrier extraction capability. For 7.5 mol% MASnCl3 added devices, the best pixel had Jsc = 16.64 mA cm−2,Voc = 0.49 V, and FF = 65.85%. The device efficiency was η = 5.38% for an area of 0.1 cm2.

To demonstrate the potential for large-area devices, 50 mm × 50 mm substrates were used to make another batch using optimized parameters from the results shown above. We first performed photoluminescence imaging (PLI) on the ITO/PEDOT[thin space (1/6-em)]:[thin space (1/6-em)]PSS/FASnI3 films. The results are shown in Fig. S10. The uniform PL intensity distribution suggests a uniform FASnI3 film was formed from the slot-die coating on the large substrate. A batch of devices was subsequently fabricated with a 1 cm2 and 5 cm2 device area. For the champion pixels, 1 cm2 pixel demonstrated values of Jsc = 20.1 mA cm−2, Voc = 0.42 V, FF = 45.7% and η = 4.02%, while a 5 cm2 pixel demonstrated Jsc = 15.83 mA cm−2, Voc = 0.44 V, FF = 32.68%, and η = 2.31%. The low FF was attributed to the lack of an optimised testing setup, as two crocodile clips were used to make contact, leading to poor charge extraction during the measurement. Nevertheless, both PLI and solar cell performances demonstrated the potential and reproducibility for large-area FASnI3 deposition with the slot die coating technique, especially considering that the large-area devices were fabricated at a different laboratory with different equipment compared to the smaller 0.1 cm2 slot die coated devices.

Slot-die coated Sn-perovskite PV for indoor applications

One possible application for printed Sn perovskites is indoor PV, where its potentially lower toxicity compared to Pb perovskites can be beneficial. We tested the FASI-MASnCl3 devices with different MASnCl3 concentrations using LED light to simulate indoor conditions. As shown in Fig. 4, FASI-7.5 mol% MASnCl3 exhibited the best performance across a range of light intensities. At 0.03 sun, it obtained η = 5.4%. Fig. S11 presents the Voc changes at the LED intensities studied. The combination of a lead-free device and deposition via slot die coating is a promising breakthrough for indoor PV applications.
image file: d4se01321b-f4.tif
Fig. 4 (a) Spectrum of the LED used to test indoor PV performance and (b) the corresponding PCE under different light intensities for FASI with different mol% concentration of MASnCl3.

Conclusion

Sn perovskite solar cell efficiencies have increased significantly recently and are now reaching 14%. However, roll-to-roll printing of FASnI3 solar cells has not yet been achieved. Here, we address the key challenge of uncontrolled crystallization in this material to successfully print Sn-perovskite solar cells via slot-die coating. A novel crystallization approach was applied with a combination of solvent and additive engineering and a gas pulse trigger for Sn perovskite nucleation in the slot-die-coated wet films. FASnI3 films were coated on different area substrates using a DMF[thin space (1/6-em)]:[thin space (1/6-em)]tBP solvent mixture, avoiding the use of oxidative DMSO while slowing down crystallisation via a tBP-based intermediate phase. The rate of crystallization was controlled using the additives SnCl2, SnF2, MACl, and MASnCl3. In situ PL and transmission measurements performed during and after gas pulsing showed that finding an optimal kinetics of nucleation is extremely beneficial for producing high quality solar cell devices. The best perovskite films were fabricated with MASnCl3 as an additive, showing intermediate crystallisation kinetics amongst the studied systems, leading to a pinhole-free morphology, highest PLQY. This result is consistent with the need to create a Sn-rich environment to compensate for Sn vacancy defects and minimize Sn2+ oxidation during crystallisation, and the usefulness of Cl to favourably direct crystal growth and in improving charge collection, and the role of MA+ in slowing down crystallisation through intermediate adduct formation. Optimisation of the FASI-MASnCl3 composition led to the fabrication of devices achieving η = 5.38% for 0.1 cm2 and η = 4.02% for 1 cm2 and η = 2.31% for 5 cm2 device area. The device was also tested under indoor light conditions and demonstrated a similarly high performance. Therefore, we report the first lead-free Sn perovskite solar cells achieved via an antisolvent-free and entirely scalable method that is suitable for roll-to-roll production, demonstrating the potential of this technology for future PV applications.

Methods section

Materials

Unless otherwise specified, the chemicals were used as received without further purification. Tin(II) iodide (SnI2), ethylenediammonium diiodide (EDAI2, >98%), N,N-dimethylformamide (anhydrous, 99.8%), 4-(tert-butyl) pyridine (98%), bathocuproine (BCP), and silver beads were purchased from Sigma-Aldrich and used as received. Formamidinium iodide (FAI, >98%) was purchased from Dyenamo. Patterned ITO glass slides were purchased from Ossila. PEDOT[thin space (1/6-em)]:[thin space (1/6-em)]PSS polymer dispersion in both water and toluene (CLEVIOS™) was purchased from Heraeus.

Perovskite solution preparation

A solution of SnI2 was dissolved in pure DMF first. The solution was kept under shaking at ambient temperature for one hour to dissolve the tin salts completely. FAI powder was scaled in a new vial, and the proper amount of the SnI2 solution was added to the powder, leading to a desired FA[thin space (1/6-em)]:[thin space (1/6-em)]Sn molar ratio. The solution was kept under shaking for an hour at ambient temperature for the complete dissolution of FAI. Afterwards, tBP was added to achieve the desired volume ratio between DMF and tBP (6[thin space (1/6-em)]:[thin space (1/6-em)]4 for slot die coating). EDAI2, SnCl2 and MASnCl3 were dissolved in separate vials with pure DMF to make a 1M stock solution. MACl and SnF2 were added as powers due to poor solubility in DMF. Finally, the FASnI3 solution (0.6 M for slot die coating) with different additives was achieved by adding the corresponding additives and further shaking for one hour. All additives were 2.5 mol% in the final solutions. For the investigation of MASnCl3 concentration, five solutions were prepared: 2.5 mol%, 5 mol%, 7.5 mol%, 10 mol% and 12.5 mol%. The solution was filtered with a 0.2 μm PTFE filter before use.

Solar cells fabrication

An inverted structure was chosen for the PSCs fabricated with the following stacking: glass/ITO/PEDOT[thin space (1/6-em)]:[thin space (1/6-em)]PSS/FASnI3/C60/BCP/Ag. Patterned indium tin oxide (ITO) coated glasses were first washed in an ultrasonic thermal bath at 40 °C with the following procedure: 15 minutes with a liquid detergent dissolved in deionised water (2% V/V); rinsed in deionised water and sonicated for 5 minutes; rinsed in acetone and then sonicated for 15 minutes; rinsed in ethanol and then sonicated for 15.

For slot die coating, clean substrates were treated using UV ozone cleaner (Ossila) and aqueous PEDOT was deposited in ambient conditions. The deposition remained the same. Films were annealed at 120 °C for 20 min. After moving the substrates into the glovebox, substrates were placed on a slot die coater (Ossila) for perovskite deposition. The stage was kept at 40 °C during the coating. The moving speed was set at 5 mm s−1; the dispense rate was set at 1 μL s−1. After the coating, the substrate was removed from the stage, and a handheld air blow gun was used to blow the surface at a distance of 10 cm quickly. Ideally, an automated air knife could be fitted inline so the gas pulse happens during the coating. This could not be achieved because the stage has no vacuum suction function to fixate the substrate or enough coating distance (maximum 10 cm) to fit the air knife. After the quick blow, the film turned red and was immediately placed onto a hot plate for annealing at 140 °C for 20 min.

The gas blow was applied with a 5 bar N2 gas gun in the glovebox from a 10 cm distance above for all perovskite deposition experiments.

The ETL and the silver electrode were deposited using a thermal evaporation chamber at a high vacuum (<10−6 bar). The thickness of the three layers, C60, BCP and Ag, were 75, 7 and 150 nm, respectively.

For slot die coating of large area (50 × 50 mm) devices, the process was repeated at a different lab with same deposition parameters. All equipment remained the same except the slot die coating was performed on the larger FOM alphaSC slot die coater and a Keithley 2400 was used for measurement with a WAVELABS Sinus LED solar simulator.

In situ PL and transmission measurement

The in situ PL and transmission measurement was conducted in a N2-filled glovebox. The excitation was provided by Avantes portable LED laser (AvaLight-HPLED, 3.4 mW, 405 nm). A Wasatch f/2 high throughput spectrometer (WP-VISNIR-R-S-50) captured the PL response. Thorlabs Reflection probe RP23 was used for the measurement at reflection mode. For transmission, Avantes AvaLight-DHc was used as light source, Avantes AvaSpec-ULS2048CL-EVO was used as the spectrometer, SMA-905 optic fibres and M6 tapped optical breadboards were purchased from Thorlabs. The set-up is illustrated in Fig. S3.

PLQY measurement

The photoluminescence quantum yield was measured with a calibrated Quantum Yield Berlin LuQY Pro setup. The samples were illuminated in an integrating sphere with a 532 nm laser with intensities between 0.05 and 1 sun equivalence. For each illumination intensity, five spectra were recorded and averaged.

Photovoltaic characterisation

The multimodal Arkeo machine from Cicci Research s.r.l. was used to characterise the solar cell performance in the glovebox. The device's current density–voltage (JV) characteristics were tested using a 12 LED solar simulator with a calibrated optical power density of 100 mW cm−2. PSC JV characteristics were measured every 10 mV with a sample rate of 100 mV s−1. Incident photon to current conversion efficiency (IPCE) were measured using a commercial apparatus (Arkeo-Ariadne, Cicci Research s.r.l.) based on a 300 Watt Xenon lamp. The monochromatic light intensity was calibrated using a Hamamatsu S1337 Si-calibrated photodiode.

Structural characterisation

Scanning electron microscopy (FEI inspect F) was used for observing perovskite morphology and device architecture. X-ray diffraction was performed using a Siemens D5005 diffractometer from 5° to 70° using Cu Kα radiation. Crystal peaks were identified using the International Centre for Diffraction Data (ICDD) database.

Photoluminescence imaging (PLI)

PL imaging was done with a camera using a silicon CCD detector. As excitation source an array of 520 nm LEDs were used to provide homogeneous illumination over the whole imaged area. The integration time was optimized for each sample to make maximal use of the 16 bit dynamic range of the CCD detector. Additionally, a 700 nm long pass and an 850 nm short pass filter were used between sample and camera.

Data availability

All data from the manuscript, scalable slot-die printing of lead-free tin perovskite solar cells via controlled crystallization, is freely available upon request from the authors.

Conflicts of interest

The authors declare no conflict of interest.

Acknowledgements

This work was funded by EP/V010913/1, and supported by the Italian Ministry of Environment and Energy Security in the framework of the Operating Agreement with ENEA for Research on the Electric System.

References

  1. A. Abate, Perovskite solar cells go lead free, Joule, 2017, 1, 659–664 CrossRef CAS.
  2. N. K. Noel, et al., Lead-free organic–inorganic tin halide perovskites for photovoltaic applications, Energy Environ. Sci., 2014, 7, 3061–3068 RSC.
  3. F. Hao, C. C. Stoumpos, D. H. Cao, R. P. H. Chang and M. G. Kanatzidis, Lead-free solid-state organic–inorganic halide perovskite solar cells, Nat. Photonics, 2014, 8, 489–494 CrossRef CAS.
  4. J. Chen, et al., Spatially isomeric fulleropyrrolidines enable controlled stacking of perovskite colloids for high-performance tin-based perovskite solar cells, Angew. Chem., Int. Ed., 2025, e202420150 CAS.
  5. M. De Bastiani, et al., Monolithic perovskite/silicon tandems with >28% efficiency: role of silicon-surface texture on perovskite properties, Adv. Funct. Mater., 2023, 33, 2205557 CrossRef CAS.
  6. Best Research-Cell Efficiency Chart | Photovoltaic Research, NREL, https://www.nrel.gov/pv/cell-efficiency.html Search PubMed.
  7. J. Wang, et al., Controlling the crystallization kinetics of lead-free tin halide perovskites for high performance green photovoltaics, Adv. Energy Mater., 2021, 11, 2102131 CrossRef CAS.
  8. T. Wu, et al., Lead-free tin perovskite solar cells, Joule, 2021, 5, 863–886 CrossRef CAS.
  9. H. Dong, et al., Crystallization dynamics of sn-based perovskite thin films: toward efficient and stable photovoltaic devices, Adv. Energy Mater., 2022, 12, 1–28 Search PubMed.
  10. F. Li, et al., A cation-exchange approach for the fabrication of efficient methylammonium tin iodide perovskite solar cells, Angew. Chem., Int. Ed., 2019, 58, 6688–6692 CrossRef CAS PubMed.
  11. P. Wang, et al., Ion exchange/insertion reactions for fabrication of efficient methylammonium tin iodide perovskite solar cells, Adv. Sci., 2020, 7, 1903047 CrossRef CAS PubMed.
  12. G. Nasti, et al., Pyridine controlled tin perovskite crystallization, ACS Energy Lett., 2022, 7, 3197–3203 CrossRef CAS PubMed.
  13. K. P. Marshall, M. Walker, R. I. Walton and R. A. Hatton, Enhanced stability and efficiency in hole-transport-layer-free CsSnI3 perovskite photovoltaics, Nat. Energy, 2016, 1, 1–9 Search PubMed.
  14. S. Gupta, D. Cahen and G. Hodes, How SnF2 impacts the material properties of lead-free tin perovskites, J. Phys. Chem. C, 2018, 122, 13926–13936 CrossRef CAS.
  15. S. J. Lee, et al., Fabrication of efficient formamidinium tin iodide perovskite solar cells through SnF2-pyrazine complex, J. Am. Chem. Soc., 2016, 138, 3974–3977 CrossRef CAS PubMed.
  16. M. Xiao, et al., Tin-based perovskite with improved coverage and crystallinity through tin-fluoride-assisted heterogeneous nucleation, Adv. Opt. Mater., 2018, 6, 1700615 CrossRef.
  17. B. B. Yu, et al., Synergy effect of both 2,2,2-trifluoroethylamine hydrochloride and SnF2 for highly stable FASnI3−xClx perovskite solar cells, Sol. RRL, 2019, 3, 1800290 CrossRef.
  18. M. E. Kayesh, et al., Enhanced photovoltaic performance of FASnI3-based perovskite solar cells with hydrazinium chloride coadditive, ACS Energy Lett., 2018, 3, 1584–1589 CrossRef CAS.
  19. L. He, et al., Efficient anti-solvent-free spin-coated and printed sn-perovskite solar cells with crystal-based precursor solutions, Matter, 2020, 2, 167–180 CrossRef.
  20. W. Żuraw, et al., Large-area, flexible, lead-free sn-perovskite solar modules, ACS Energy Lett., 2023, 8, 4885–4887 CrossRef PubMed.
  21. F. Xu, et al., Potassium thiocyanate-assisted enhancement of slot-die-coated perovskite films for high-performance solar cells, Small Sci., 2021, 1, 2000044 CrossRef CAS.
  22. J. Li, et al., 20.8% slot-die coated MAPbI3 perovskite solar cells by optimal DMSO-content and age of 2-ME based precursor inks, Adv. Energy Mater., 2021, 11, 2003460 CrossRef CAS.
  23. A. S. Subbiah, et al., High-performance perovskite single-junction and textured perovskite/silicon tandem solar cells via slot-die-coating, ACS Energy Lett., 2020, 5, 3034–3040 CrossRef CAS.
  24. M. Du, et al., High-pressure nitrogen-extraction and effective passivation to attain highest large-area perovskite solar module efficiency, Adv. Mater., 2020, 32, 2004979 CAS.
  25. T. Bu, et al., Lead halide-templated crystallization of methylamine-free perovskite for efficient photovoltaic modules, Science, 2021, 372, 1327–1332 CrossRef CAS PubMed.
  26. C. B. Whitehead, S. Özkar and R. G. Finke, LaMer's 1950 model of particle formation: a review and critical analysis of its classical nucleation and fluctuation theory basis, of competing models and mechanisms for phase-changes and particle formation, and then of its application to silver halide, semiconductor, metal, and metal-oxide nanoparticles, Mater. Adv., 2021, 2, 186–235 CAS.
  27. S. Kolahgar-Azari, et al., Semicrystalline polymer micro/nanostructures formed by droplet evaporation of aqueous poly(ethylene oxide) solutions: effect of solution concentration, Langmuir, 2022, 38, 15063–15076 CrossRef CAS PubMed.
  28. A. R. Pascoe, et al., Directing nucleation and growth kinetics in solution-processed hybrid perovskite thin-films, Sci. China Mater., 2017, 60, 617–628 CrossRef CAS.
  29. D.-K. Lee, K.-S. Lim, J.-W. Lee and N.-G. Park, Scalable perovskite coating via anti-solvent-free Lewis acid–base adduct engineering for efficient perovskite solar modules, J. Mater. Chem. A, 2021, 9, 3018–3028 RSC.
  30. T.-B. Song, et al., Dynamics of antisolvent processed hybrid metal halide perovskites studied by in situ photoluminescence and its influence on optoelectronic properties, ACS Appl. Energy Mater., 2020, 3, 2386–2393 CrossRef CAS.
  31. M. Kim, et al., Methylammonium chloride induces intermediate phase stabilization for efficient perovskite solar cells, Joule, 2019, 3, 2179–2192 CAS.
  32. D. J. Kubicki, et al., Local structure and dynamics in methylammonium, formamidinium, and cesium tin(II) mixed-halide perovskites from 119Sn solid-state NMR, J. Am. Chem. Soc., 2020, 142, 7813–7826 CrossRef CAS PubMed.
  33. C. M. Tsai, et al., Formation of stable tin perovskites co-crystallized with three halides for carbon-based mesoscopic lead-free perovskite solar cells, Angew. Chem., Int. Ed., 2017, 56, 13819–13823 CrossRef CAS PubMed.
  34. M. Ozaki, et al., Solvent-coordinated tin halide complexes as purified precursors for tin-based perovskites, ACS Omega, 2017, 2, 7016–7021 CrossRef CAS PubMed.
  35. T. Huang, et al., Performance-limiting formation dynamics in mixed-halide perovskites, Sci. Adv., 2021, 7, 1799 CrossRef PubMed.
  36. F. Wang, et al., 2D-quasi-2D-3D hierarchy structure for tin perovskite solar cells with enhanced efficiency and stability, Joule, 2018, 2, 2732–2743 CrossRef CAS.
  37. T.-B. Song, et al., Dynamics of antisolvent processed hybrid metal halide perovskites studied by in situ photoluminescence and its influence on optoelectronic properties, ACS Appl. Energy Mater., 2020, 3, 2386–2393 CrossRef CAS.
  38. T. Moot, et al., CsI-antisolvent adduct formation in all-inorganic metal halide perovskites, Adv. Energy Mater., 2020, 10, 1–9 Search PubMed.
  39. T.-B. Song, et al., Revealing the dynamics of hybrid metal halide perovskite formation via multimodal in situ probes, Adv. Funct. Mater., 2020, 30, 1908337 CrossRef CAS.
  40. V. K. LaMer and R. H. Dinegar, Theory, production and mechanism of formation of monodispersed hydrosols, J. Am. Chem. Soc., 1950, 72, 4847–4854 CrossRef CAS.
  41. P. G. Vekilov, The two-step mechanism of nucleation of crystals in solution, Nanoscale, 2010, 2, 2346–2357 RSC.
  42. C. Liu, Y. B. Cheng and Z. Ge, Understanding of perovskite crystal growth and film formation in scalable deposition processes, Chem. Soc. Rev., 2020, 49, 1653–1687 RSC.
  43. C. Liu, Y. B. Cheng and Z. Ge, Understanding of perovskite crystal growth and film formation in scalable deposition processes, Chem. Soc. Rev., 2020, 49, 1653–1687 RSC.
  44. R. L. Milot, et al., The effects of doping density and temperature on the optoelectronic properties of formamidinium tin triiodide thin films, Adv. Mater., 2018, 30, 1804506 CrossRef PubMed.
  45. E. Jokar, et al., Slow surface passivation and crystal relaxation with additives to improve device performance and durability for tin-based perovskite solar cells, Energy Environ. Sci., 2018, 11, 2353–2362 RSC.
  46. S. Shao, et al., Highly reproducible sn-based hybrid perovskite solar cells with 9% efficiency, Adv. Energy Mater., 2018, 8, 1702019 CrossRef.
  47. Z. Chen, et al., Thin single crystal perovskite solar cells to harvest below-bandgap light absorption, Nat. Commun., 2017, 8, 1890 CrossRef PubMed.
  48. Y. Lei, et al., A fabrication process for flexible single-crystal perovskite devices, Nature, 2020, 583, 790–795 CrossRef CAS PubMed.
  49. Y. Takahashi, H. Hasegawa, Y. Takahashi and T. Inabe, Hall mobility in tin iodide perovskite CH3NH3SnI3: evidence for a doped semiconductor, J. Solid State Chem., 2013, 205, 39–43 CrossRef CAS.
  50. D. B. Mitzi, C. A. Feild, Z. Schlesinger and R. B. Laibowitz, Transport, optical, and magnetic properties of the conducting halide perovskite CH3NH3SnI3, J. Solid State Chem., 1995, 114, 159–163 CrossRef CAS.
  51. M. Stolterfoht, et al., The impact of energy alignment and interfacial recombination on the internal and external open-circuit voltage of perovskite solar cells, Energy Environ. Sci., 2019, 12, 2778–2788 RSC.
  52. C. M. Wolff, et al., Nonradiative recombination in perovskite solar cells: the role of interfaces, Adv. Mater., 2019, 31, 1902762 CrossRef CAS PubMed.
  53. P. Caprioglio, et al., On the relation between the open-circuit voltage and quasi-fermi level splitting in efficient perovskite solar cells, Adv. Energy Mater., 2019, 9, 1901631 CrossRef.
  54. J. Warby, et al., Mismatch of quasi–fermi level splitting and Voc in perovskite solar cells, Adv. Energy Mater., 2023, 13, 2303135 CrossRef CAS.
  55. W. Liu, et al., Tin halide perovskite solar cells with open-circuit voltages approaching the shockley-queisser limit, ACS Appl. Mater. Interfaces, 2023, 15, 32487–32495 CrossRef CAS PubMed.
  56. J. Warby, et al., Understanding performance limiting interfacial recombination in pin perovskite solar cells, Adv. Energy Mater., 2022, 12, 2103567 CrossRef CAS.

Footnotes

Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4se01321b
Authors contributed equally.

This journal is © The Royal Society of Chemistry 2025
Click here to see how this site uses Cookies. View our privacy policy here.