Rahul Verma‡
,
Surendra K. Yadav‡,
Diksha Singh and
Jay Singh*
Department of Chemistry, Institute of Science, Banaras Hindu University, Varanasi, 221005, Uttar Pradesh, India. E-mail: jaysingh.chem@bhu.ac.in; jaimnnit@gmail.com; Tel: +91-9871766453
First published on 27th February 2025
A hydrothermally synthesized mesoporous CoFe2O4 (CF)/reduced graphene oxide (rGO) nanohybrid (nh) provides the electroactive surfaces and facilitates fast electron transfer between the nanofabricated bioelectrode–electrolyte interfaces, responsible for the high electrocatalytic activity in sensing adrenaline (AD). A promising biosensor for detecting adrenaline and bovine serum albumin (BSA) used as a real sample for diagnosing neurodegenerative diseases is described here. This study focuses on the electrochemical impedance biosensing of AD because of its unique ability to identify various kinds of health issues, including blood pressure, fight-or-flight response, memory loss, multiple sclerosis, Parkinson's disease, and cardiac asthma. A La/CF/rGO/ITO bioelectrode (La: Laccase) is the biosensor component. It is created by electrophoretic deposition (EPD) of a CF/rGO nh and drop-casting immobilization of the La-enzyme. The low charge-transfer resistance (Rct) of the CF/rGO electrode was sensed by electrochemical impedance spectroscopy (EIS), confirming the synergistic impact of CF/rGO on the La/CF/rGO/ITO fabricated bioelectrode in AD detection. This gives the high heterogeneous rate constant (Ks: 2.83 × 10−4) and increases the surface adsorption and diffusion coefficient (D: 5.25 × 10−2 cm2 s−1). The proposed biosensor exhibited high sensitivity (0.214 Ω μM−1 cm−2), long linear range (1 to 500 μM), lower detection limit (LoD: 40.3 μM), high selectivity (RSD 5.8%), and stability with good recovery %, emphasizing its potential implementation in biosensing techniques for monitoring neurotransmitter disorders in real world applications.
The scientific and engineering communities have been drawn to graphene, a remarkable 2D sp2 – hybridized carbon material, because of its unique qualities, such as large surface area, mechanical strength, thermal stability, ultra-thin nanostructure, and excellent electrical conductivity (faster carrier mobility). Graphene has become attractive as an electrode material for use in electrochemical applications, like sensors/biosensors, supercapacitors, and catalysis with promising potential applications.21–23 Graphene sheets have finite dimensions and morphological characteristics such as dislocation, edge defects, and rings with five to eight members that resemble hexagons and honeycombs, attached via van der Waals and π–π weak interactions. Reduced graphene oxide (rGO) and graphene oxide (GO) are two significant derivatives of graphene. rGO exhibits increased electrical conductivity because of the removal of oxygen-holding carboxyl groups (COOH) present on the basal plane and edges of the crystal lattices. The significance of rGO focused on in this article is special characteristics like its optical, mechanical, thermal, surface area, and electrical characteristics which have extensive usefulness such as in photocatalysts,24 energy storage, catalysis, solar cells,25 biosensors/sensors,26 hybrid materials, and electronic devices as ideal materials for electrochemical applications.27,28 Furthermore, superior dispersibility and hydrophilicity in aqueous media mainly depend on groups such as COOH, OH, and the epoxy moiety on the surface of rGO.29,30 However, these groups on the surface of rGO also limit its electrical conductivity, which makes it difficult to directly use rGO in electrode materials and devices. As a result, to facilitate its direct deployment, the topic of restricted electrical conductivity in rGO needs attention. The goal of recent research has been to understand better how to improve rGO electro-conductive capabilities for a range of analytes by incorporating metal/ferrite oxide hybrid materials by enhancing the rGO electrical conductivity to utilize the mixed nh (Ferrites) materials in several electrode material and electronic device applications.31,32 Thus, using techniques like doping, chemical modification, and nh synthesis with other materials has been enhancing the electrocatalysis of rGO.33–35
Nanoparticles (NPs) of transition metal oxides have emerged with fascinating potential for a range of potential applications like water purification, energy conversion, fuel cells, sensors, and storage.36 Because of these NPs’ redox activity, nontoxicity, high stability, affordability, environmentally friendly nature, and natural abundance, researchers studying electrocatalysis have been keenly interested in them.37–39 However, individual metal oxides’ poor conductivity has restricted their practical application. The use of mixed transition metal oxide NPs has been investigated as a solution to this constraint. Because these NPs combine two distinct metal species into one crystal structure, they have mixed valency and can facilitate a variety of redox processes.36 Additionally, by combining these mixed metal oxides with pure metal oxides in a synergistic way, the effectiveness of the electrocatalytic reaction can be improved, leading to a wider range of working potentials, better conductivity, more electroactive sites, and increased stability. Because of their improved physical and chemical qualities over traditional bulk materials, magnetic NPs have been trendsetting in recent years.40–42 Ferrites are a class of magnetic NP materials with significant technological value and a wide range of applications, including biosensing.19,43 To monitor neurotransmitters and epinephrine concurrently using an electrochemical approach, Roychoudhury et al. used the NiO/rGO platform.44 Therefore, in the electrochemical monitoring of bio-analytes, the combination of CF and rGO offers promising candidates with exceptional catalytic and conductive efficiency.
After applying the produced nanohybrid (nh) to the ITO surface, the modified CF/rGO/ITO electrode is subjected to the drop-cast approach to optimize the immobilization of the laccase (La) enzyme. Because of the many active sites and efficient, fast electron transport mechanisms in the mesoporous CF/rGO nh on modified ITO (La/CF/rGO/ITO), enhanced sensing signals can be generated to evaluate AD selectively. Compared to the CF/ITO pretreatment, the CF/rGO-modified electrode shows a larger effective surface area and electrocatalytic efficiency in favor of AD. We conclude that the CF/rGO nh is a promising material for biosensing applications using electrochemical techniques. Based on our knowledge, no earlier report was found on novel La/CF/rGO/ITO bioelectrodes for AD monitoring by EIS techniques. The low-temperature hydrothermally synthesized CF/rGO nh are electrophoretically deposited and enzyme immobilized on their surface to investigate the AD selectively, enhancing the active sites with surface area for binding and fast charge transfer reaction. In addition, the fabricated bioelectrode detects the AD with a more extended linear range, lower detection limit (LoD), stability, and high sensitivity and was applied to the real (BSA) sample with relative standard deviations (RSD 8.3%) recorded. These results make the CF/rGO unique compared to traditional materials that offer several advantages in monitoring neurotransmitters important to neurological disorders and healthcare monitoring.
Mesoporous cobalt ferrite NPs were hydrothermally synthesized from salts of Co(NO3)2·6H2O (0.4 M aqueous solution) and Fe(NO3)3·9H2O (0.8 M aqueous solution) as precursors (1:
2 ratio of concentration) in 50 ml solution, while stirring for 2 h (1200 rpm) at 60 °C. After that, 100 mg GO sheets were used to prepare a solution in 25 ml distilled water after 35 minutes of ultrasonication. Then, the GO solution and salt solution were mixed for 2 h with the same stirring speed, and the pH of the solution was found to be five. In the later step, the NH3 solution of 25% was added, with surfactant oleic acid (2 ml, for nucleation and high crystallinity); the pH reached up to 9 to start the conversion from nitrate salt solution to metal hydroxide (Fe/Co–OH) solution at 60 °C and with stirring for 3 h. In addition, the mixture of the blackish solution was placed in Teflon-lined stainless auto-clave vessels (100 ml) and synthesized at 180 °C for 20 h. After completing the hydrothermal reactions, the autoclave was cooled, the solution was centrifuged in a water/ethanol mixture, dried at 90 °C overnight, and then calcined at 400 °C for 6 h. The resulting powder was confirmed by XRD and Raman analysis as a CF/rGO nh,46 and a schematic presentation of the hydrothermal synthesis is represented in Scheme S1 (ESI†). An equivalent approach was also applied in the preparation of CF NPs using a hydrothermal method without the addition of GO in the reaction conditions, and these prepared mesoporous CF/rGO nh materials were used to fabricate electrodes for electrochemical monitoring of AD neurotransmitters.
a = λ (h2 + k2 + l2)1/2/2![]() ![]() | (1) |
D = 0.9λ/β![]() ![]() | (2) |
ρ = nM/NAa3 | (3) |
The λ is the wavelength of the X-ray, the miller indices are h, k, and l of the plane (311 planes of high intensity), θ is the Bragg diffraction angle in radians, β is the full width at half maximum (FWHM) in radians, n is the number of atoms/molecules (8 in spinel) participating in the lattice structure, M is the molecular weight of the prepared materials, and NA is Avogadro's number (6.02 × 1023 mol−1).
The XRD peak broadening is a consequence of lattice strain and small particle size. This principle underpins several techniques, including the Scherrer equation, Hall–Williamson method, and the Warren–Averbach method. In this study, the Hall–Williamson method was used to estimate lattice strains, eqn (S1) (ESI†). Fig. S1(A and B) (ESI†) shows a positive slope of the strain curve for CF/rGO (0.00097) and CF (0.00159) indicating the presence of tensile strain in the lattice. As a result, both lattice strain and the observed Debye–Waller factor increase. Debye temperatures are calculated using the zero-strain values of the Debye–Waller factor.48 The Debye temperature (TD) varies as a function of the band gap (Eg) of the material, following the relationship TD ∝ exp(Eg).49 Consistent with this trend, the tensile strain in CF is greater than that in CF/rGO, leading to a larger band gap (calculated band gap value from UV-vis data) and, consequently, is well-aligned with the CV curve as well.
The local distortion and cation distribution can be determined using Raman spectroscopy. The spinel of rGO, CF, and CF/rGO nh is shown in Fig. 1B, revealing a sharp and intense absorption band signifying their high crystallinity. High-performance charged coupled device detectors (Horiba LabRam HR evolution spectrometer) use a 633 nm He–Ne beam illuminating the sample in the 200–3500 cm−1 range. The inverse spinel structured materials have Co2+ cation occupying the octahedral (Oh) sites and Fe3+ cations in half of the Oh sites and half of the tetrahedral (Td) sites. Furthermore, the CF has a cubic face-centered structure containing space group Fdm, and 56 atoms (Z = 8) in one complete unit cell50 analysis to predict the spinel modes;
Γ = Eg (R) + A1g (R) + T1g + 3T2g (R) + 2A2u + 2Eu + 4T1u (IR) + 2T2u |
Fourier-transform infrared (FTIR) spectroscopy reveals the functionalization and location of surface groups in CF and CF/rGO nh detected in the range of 400 to 3500 cm−1 (JASCO-FTIR-4700). Fig. 1C shows the vibrational bands between 420 cm−1 to 580 cm−1 are related to the Td (Co–O) and Oh (Fe–O) rearrangement of cation sites respectively, to confirm the formation of inverse spinel ferrite.20 The stretching mode of symmetric and antisymmetric peaks of C–H at 2900–2950 indicates the polymer matrix rGO with 1220 (C–C), 1670 (CO), and 2320 (COOH) peaks containing functional groups.43 The carbonyl group, epoxy, and carboxylic groups confirm the formation of CF/rGO nh, supporting the final results of the XRD analysis.
The optical behavior of rGO, CF, and CF/rGO nh was inspected by UV-vis absorption spectroscopy from 200 to 400 nm wavelength (UV-1700 pharma Spec, SHIMADZU, D2, and W lamp). Fig. 1D shows that the absorption spectra of the hydrothermally prepared rGO, CF, CF/rGO nh is ∼265 nm. Furthermore, these results are utilized to calculate the change in the samples’ energy gap (band gap Eg) by using the Tauc relationship,53 which is given in eqn (4).
α = K(hν − Eg)n/hν | (4) |
Here α is the absorption coefficient, K is a constant (K ∼ 1), hν is the photon energy (hν = 1240 eV), and n is the direct transition in the semiconductor (1/2). The plot of (αhν)2 versus hν is used to determine the direct band gap of the proposed materials. Thus, the rGO, CF, and CF/rGO nh have direct optical band gaps of 4.22, 4.16, and 4.07 eV, respectively, after Tauc plot analysis. These results reveal that the rGO addition in the nh decreases the electron–hole band gap and enhances the charge transfer activity of the CF/rGO nh. Thus, the lower energy gap in nh materials caused the insulators to exhibit semiconductor behaviors, which enhances their electrical conductivity and allows them to be utilized in electrochemical biosensing applications.54
High-resolution (HR) TEM observations were performed to examine the internal shape, morphology, and crystalline nature of the mesoporous CF and CF/rGO nh. Fig. 2A depicts the CF magnetic spinel ferrite achieving a uniform rectangular and rhombus mix-phase parallelogram morphology. Furthermore, the investigation of lattice fringes in CF is seen in the HR-TEM image, Fig. 2B. The JCPDS file confirms lattice spacing (0.25 nm) equivalent to the high-intensity plane (311). Thus, the SAED pattern of CF indexed (Fig. 2C), which is like the Debye–Scherrer pattern of CF indexed (620, 511, 422, and 220) planes, confirms the polycrystalline nature of the materials. The CF/rGO nh HR-TEM images show the spherical as well as rectangular morphology and lattice plane, also showing d-spacing (0.25 nm) equivalent to the high intensity 311 plane, and the similar spacing circular SAED pattern confirms the polycrystalline nature of the nh material (Fig. 2D–F). The CF and CF/rGO nh average particle sizes calculated by applying the Lorentzian function in the Image-J software were found to be 21 nm and 19.5 nm, respectively. Relative to lattice fringes in HRTEM images, the dominant plane in XRD d-spacing confirms the high crystallinity of the proposed materials applied for electrochemical analysis.
The surface micrograph of the proposed materials is evaluated by scanning electron microscopy (SEM) (model: ZEISS, EVO-18, and LaB6 electron source). Fig. 3A and B represent the SEM micrograph of CF, which are spherical agglomerated uniform particles and corresponding energy dispersive X-ray (EDX) profiles with elements’ atomic percentages to confirm the prepared materials are CF NPs. In Fig. 3C, the addition of rGO in the CF decreases the agglomeration of spherical NPs due to the rGO sheet distributed between the CF NPs and prevents aggregation. In addition, the nh formed a large void of great benefit in the reaction interface. The output obtained thus validates the intercalation of CF on the rGO surface to increase the specific surface area (which is further validated by BET analysis in Fig. 4B) for use in electrochemical biosensing applications. The EDX analysis and composition of elements present in the prepared nanohybrid material are shown in Fig. 3D. The nh material exhibits the atomic percentages of the components Co, Fe, O, and C to prove the composition of the synthesized materials and support the XRD and Raman findings highlighting the presence of CF/rGO nh. Furthermore, the atomic force microscopy (AFM) analysis tapping mode was used to analyze the surface features of the CF and CF/rGO thin film on the ITO surface. Fig. S2(A and B) (ESI†) shows that the CF average roughness (Sa) is 6.3 nm, root mean square roughness (Sq) is 8.1 nm and maximum area peak height (Sp) is 33.2 nm, and Fig. S2(C and D) shows the roughness parameters of CF/rGO such as Sa is 4.3 nm, Sq is 5.6 nm, and Sp is 25.9 nm, which are discussed in the ESI† (Section 2).
![]() | ||
Fig. 3 (A) and (B) SEM micrograph of CF with EDX containing the corresponding element percentages, and (C) and (D) SEM micrograph of CF/rGO with EDX containing the corresponding element percentages. |
![]() | ||
Fig. 4 (A) The mesoporous CF and pore diameter, and (B) the mesoporous CF/rGO nh with a pore diameter of BET adsorption–desorption N2 isotherm. |
The key factors that affect the charge/ion transport in electrochemical analysis are the surface area, porosity, and pore size allocation. The larger the specific surface area and hierarchical pores the greater the number of active sites for electrochemical reactions. N2 adsorption porosimetry is frequently employed in experimental settings to characterize the specific surface area (in m2 g−1), pore size allocation, and open porosity of mesoporous materials (pore size 2 to 50 nm in range). The specific surface area of the mesoporous materials is determined by using the Brunauer–Emmett–Teller (BET) method expressed as:
BET = NmNACN2 |
X-ray photoelectron spectroscopy (XPS) was carried out on the electrostatically self-assembled CF and CF/rGO nh to confirm the elemental oxidation states, binding energy, and surface composition. The elements Co, Fe, O, and C were detected in the CF/rGO nh, which are excited by X-ray at the adjustable spot size from 10 to 200 μm, up to 1.4 mm scanning dimensions (ULVAC-PHI, INC.PHI 5000 Versa Probe-III, X-ray source AlKα, hν = 1486.6 eV) as shown by the survey spectrum illustrated in Fig. 5A. These elements were evidence of the practical unification of rGO and CF. The high-resolution peak fitting is investigated using the XPS-peak-41 software by applying the Shirley background in each element's XPS analysis. The deconvoluted high-resolution peak of the C 1s spectrum shows binding energies at 282.5–284.1 (C–C/CC), 285.7 (C–O), and 291 (C
O) eV, respectively, as shown in Fig. S3 (ESI†). The carbon atom in the GO lattice C–C/C
C signifies the sp2 hybridization, and other residual components signify the oxygen-containing entity in the rGO. Furthermore, the linear fitting background applied in the high-resolution fitted peak of Co 2p at 778 and 793.5 eV correspond to Co 2p3/2 and Co 2p1/2 and other satellite peaks at 780.4, 784.1, and 800.3 eV to describe the appearance of the Co2+ state. At the same time, the spin–orbit splitting gap is 16 eV to confirm the Co2+ oxidation state57 in the prepared material, as shown in Fig. 5B. In addition, the Shirley fitted Fe 2p spectrum gives two significant peaks at 722.6 Fe 2p1/2, and 709.2 Fe 2p3/2, eV, which confirms the Fe3+ state and the peak difference of 13 eV again validates the result of the Fe3+ state expressed in Fig. 5C. The Fe3+ in Oh and Td sites are responsible for the first and second fit peaks in spinel ferrites. Some other additional satellite peaks at 712.6 and 716.3 support the Fe3+ oxidation state.19 Fig. 5D expresses the deconvoluted O 1s peak at 527.5 eV for O−2, 528.6 eV for a metal oxygen bond, and 529.7 eV for chemically adsorbed OH/H2O species in the XPS spectrum. The spin orbit splitting of 16 eV and the triplet and singlet state energy difference of 13 eV signifies the presence of Fe3+ and Co2+ states respectively. Therefore, the results of the XPS study validate the results of the Raman and XRD analyses and confirm the elemental oxidation state of the hydrothermally synthesized nh ferrite material.
The biosensing efficiency of the enzyme depends on the surface attachment of biomolecules and the selection of a suitable pH. This allows it to interact electrostatically with oppositely charged (net positive or negative charges of biomolecule) functional groups or surfaces, resulting in enhanced binding affinity, selectivity, and sensitivity of the engineered biosensors. After that, the enzyme immobilization on a CF/rGO/ITO-modified electrode is performed using the drop cast method. Fig. 6A shows the different volumes of enzyme loading used to optimize the Rct response by using the 2, 5, 10, 15, and 20 μl solution of phosphate buffer at pH 7.0. As a result, the 5 μl solutions on the electrode surface have the lowest Rct value (197 Ω), showing the maximum current response, which is a suitable amount of enzyme to use in AD detection. The optimized La enzyme 5 μl solutions are uniformly spread out over an EPD-deposited CF/rGO/ITO electrode surface and dried overnight at room temperature for later investigations. The proposed bioelectrode La/CF/rGO/ITO is ready for further electrochemical CV and EIS analysis (CorrTest CS-350 electrochemical workstation) and stored at 4 °C.
The electrochemical characteristics of the electrodes such as ITO, CF/ITO, CF/rGO/ITO, and La/CF/rGO/ITO bioelectrodes employed in 50 mM phosphate buffer containing NaCl (0.9%), pH 6.5, ferricferro–hexacyano redox couple 5 mM, scan rate 50 mV s−1 and optimized potential range is −0.7 to 1 Volt (V) in CV analysis. After that, this reaction condition was also useful in EIS analysis with a frequency range of 100000 to 0.01 Hz (from initial to final), point/decade is 10, AC amplitude of 5 mV, and effective surface area of La/CF/rGO/ITO bioelectrode is 0.97 cm2 (calculated by using Randles–Sevcik eqn (S1) discussed in Section S2.1, ESI†). These CV and EIS-optimized electrochemical parameters are jointly denoted as OEP, and utilized in the whole electrochemical analysis.
The standard stoke solution of analyte can be prepared using the AD powder used to prepare 0.2 M concentrated solution in Milli-Q water (resistivity 15 Ω sq−1), then serial dilution to prepare the different micromolar concentrations in 1 ml. After that, the real sample (BSA) was prepared at 50 mg ml−1 in a phosphate buffer at neutral conditions by using the standard addition method. Additionally, this BSA solution was further diluted in multiples of 5, 10, 15, and 20, which were used in optimization analysis as shown in Fig. S4 (A and B) (ESI†). The lowest Rct value of the pure BSA (not diluted) was 245 Ω, used as a real sample to prepare a spike solution for AD monitoring.
The EIS data were fitted using an appropriate model resembling the sensor circuit, yielding values for Rs, charge transfer resistance (Rct), and Warburg short (Ws) as the diffusion resistance. The Rct values for ITO, (374 Ω), CF/ITO (307 Ω), CF/rGO/ITO (250 Ω), and La/CF/rGO/ITO (194 Ω) electrodes were observed at OEP, sequentially. The integration of rGO nanosheets in the nh electrode increased its electronic conductivity, and electron-transfer process, as indicated by the reduced Rct value of 250 Ω for the CF/rGO/ITO electrode. Interestingly, the La/CF/rGO/ITO electrode displayed a significantly lower charge-transfer resistance (194 Ω) compared to the others, suggesting an efficient electron conductive channel towards the bioelectrode for the current generation and significant interaction between the bioelectrode and analyte. The Randles circuit model was used to estimate the Rct values for all four electrodes, including the biosensor. Moreover, for the La/CF/rGO/ITO electrode, the Rct value was employed to calculate the heterogeneous charge transfer rate constant19 (Ks) for the redox couple by using eqn (5).58 The Ks value for the fabricated electrode ITO (1.47 × 10−4 s−1), CF/ITO (1.79 × 10−4 s−1), CF/rGO/ITO (2.19 × 10−4 s−1), and La/CF/rGO/ITO (2.83 × 10−4 s−1), respectively. The CV and EIS result shows that the prepared bioelectrode La/CF/rGO/ITO is suitable for the electrochemical monitoring of AD.
Ks = RT/n2F2ARctC | (5) |
Here R is 8.314 J mol−1 K−1 the gas constant, T = 300 Kelvin, F is the Faraday constant (96500 C mol−1), n is the number of electrons involved, A is the effective surface area, and C is the concentration of electrolyte (5 × 10−6 mol cm−3).
The pH level of its environment significantly influenced the electrical response of the enzyme–substrate interface. Specifically, the La enzyme showed an optimal pH range between 5.5 and 8.0, neutral to slightly basic. This pH range was crucial for effective interaction for enzyme–substrate binding. Additionally, variations in pH affected the AD binding to the enzyme and the Ks at the electrode surface. Extreme pH conditions, either highly acidic or alkaline, could cause degradation or corrosion of the electrode surfaces, compromising biosensor reliability. To better understand and optimize these pH effects, an experiment was conducted using a La/CF/rGO/ITO bioelectrode in a range of pH solutions (from 5.7–8.0) at an OEP. The results, displayed in Fig. 6C, highlighted the profound impact of pH on the Rct value. It was observed that at higher pH, the peak potential shifted a little toward the positive side. The peak current rose with an increase up to a pH value of 7.5 at 150 Ω and the Rct value reached saturation as the pH rose to 8.0. There is a line parallel to the X-axis, as seen between pH 5.7 and 6.0, so the optimum pH range could be 6.5 (lowest Rct value), which is close to neutral pH. Therefore, a pH of 6.5 was identified as the most effective interaction for AD monitoring, yielding a low Rct value (high electrical conductivity). Researchers must meticulously regulate and optimize the pH conditions during biosensing experiments for accurate and reliable AD detection.
The EIS technique used in response time analysis was performed in the range of 1–70 s with 5 s intervals taken after completing the analysis at OEP, using AD (100 μM, 50 μl) in phosphate buffer on the proposed La/CF/rGO/ITO bioelectrode. Thus, the maximum electrical conductivity was achieved at 30 s, which means the Rct value at this point was found to be the lowest (196 Ω) in the Nyquist plot shown in Fig. 6D. Additionally, the proposed biosensors are reliable for monitoring neurotransmitters, and 30 s response time is good for biosensing applications of standard and real sample detection of AD.
The kinetic analysis and scan rate effects of the nanofabricated La/CF/rGO/ITO electrode were investigated from 10 to 100 mV s−1 with regular intervals of 10 mV s−1, as shown in Fig. S6(A) (ESI†). The scan rate steps follow the increase of anodic/oxidation current peak (Ipa) and cathodic/reduction current peak (Ipc) due to the decrease of diffusion layer with increasing scan rate, resulting in the mass transfer process/diffusion-controlled process, and quasi-reversible nature of the bioelectrode. Fig. S6(B) (ESI†) shows the linear calibration graph between the square root of the scan rate (ν1/2) versus current (mA), which is used to calculate the kinetic parameters such as surface concentration (I*), effective surface area, and diffusion coefficient (D) discussed in the ESI† as eqn (S2) and (S3) (Section S2.2).
It has been investigated how the concentration of particular analytes in solutions relates to the impedance. The total Rs is calculated below.
Rs = Rsolution + Rd + Rcircuit+instrument |
Here, Rs is the total series resistance of the circuit, that is, the linear sum of Rsolution, Rd, and Rcircuit+instrument; terms have their self-explanatory meanings as solution resistance, diffusion resistance, and total circuit resistance present in the system, including connecting wires, respectively. The voltammograms are slightly sloped, indicative of constant phase element (CPE) behavior, which cannot be ascribed to the ohmic drop. This CPE behavior stems from a distribution of time constants, explained by the dispersion of the interfacial capacitance and solution resistance. The analysis of the capacitive current reveals nonlinear behavior consistent with a CPE highlighting the necessity of incorporating a CPE element for a realistic description of the interface. Omitting this element could lead to significant errors in capacity determination. While an ideal capacitor is expected to exhibit purely non-faradaic behavior and shift electric signals by a phase of π/2, practical observations show non-ideal behavior, with phase shifts of n·π/2, where n typically ranges from about 0.8 to 1. Due to this phase shift variation, the element is termed a CPE, which also encompasses a standard capacitor when n equals 1. Its impedance is expressed below59
Y0 and n are characteristic parameters of CPE. Here, n (0 ≤ <n ≤ 1) is an independent parameter; if n = 1, CPE becomes a geometrical pure capacitor. A CPE results in a better fitting curve than a capacitor, but its parameter Y0 does not give any relevant physical significance as the capacitor does. To convert Y0 into equivalent capacitance60
To make it worthwhile for practical application for real systems, many scientists have suggested an advanced conversion method with as the frequency where the imaginary part of impedance has its maximum, as follows61
The La/CF/rGO/ITO bioelectrode demonstrates a high affinity for the analyte AD, exhibiting a sensitivity of 0.214 Ω μM−1 cm−2. The bioelectrode can detect AD across a longer linearity of 1 to 500 μM than reported in previously published articles,1,62 as shown in Fig. 7A. The La/CF/rGO/ITO bioelectrode in detecting varying concentrations of AD was evaluated using the Rct values obtained from EIS measurements spanning a frequency range from 100000–0.1 Hz, with a stimulus of 5 mV at the OEP. The Rct values, determined after fitting the data to an appropriate model as depicted in Fig. 7B (inset), served to assess the bioelectrode's response to different AD concentrations. A Nyquist plot shows the Rct values ranging from 360 Ω to 250 Ω across different AD concentrations, indicating a linear decrease in Rct value with increasing AD concentration. This linear relationship is further supported by following the equation y(Rct) = −0.208x (μM) + 348.6 and linear regression coefficient (R2) of 0.98, which underpins the calibration of the fabricated biosensor as shown in Fig. 7B. The limits of detection [LoD = 3 × SD/sensitivity], and quantification [LoQ = 10 × SD/sensitivity], were calculated based on a signal-to-noise ratio (s/n = 3), resulting in values of 40.3 μM LoD and 134.5 μM, LoQ, respectively, with a sensitivity of 0.214 Ω Mm−1 cm−2.
The decrease in Rct value with increasing AD concentration is attributed to the higher availability of AD biomolecules for interaction with the bioelectrode surface (more active sites and surface area available), which is enhanced by the nh's high surface area (119.2 m2 g−1) confirmed by BET analysis. These electrostatic interactions (positive charge on metal ions and negatively charged oxygen-containing analyte on the electrode surface) facilitate conductive pathways for electron transfer, reducing Rct and improving charge transfer efficiency. The high electrical conductivity and more binding sites at the fabricated bioelectrode interface (La and nh) are the causes of this effect. The sensitive diagnosis of AD via EIS is made possible by these specific advantages. The synergistic effect between the La enzyme and mesoporous CF/rGO nh, and the effective electrochemical reaction of AD at the bioelectrode surface are shown in Scheme 1. This nh boosts electrochemical performance by creating a conductive microenvironment, La facilitates charge transfer and the bioelectrode improves the electrode's surface area and electronic conductivity for AD oxidation. Effective electrocatalysis and variations in EIS parameters result from these interactions, making it possible to quantify and analyze AD concentrations. This has great potential for use in healthcare monitoring and diagnostics.
The reusability of the proposed AD biosensor was evaluated through 14 consecutive tests conducted in a 10 ml phosphate buffer, which included 50 μl of an 80 μM AD solution at OEP. The Rct value consistently recorded was 210 ± 4 Ω, with less than 3.16% relative standard deviation (RSD). Furthermore, the high reusability of the fabricated bioelectrode is due to the effective interaction between the La/CF/rGO/ITO bioelectrode and the La enzyme present on the electrode surface. This demonstrates the biosensor's capacity for repeated use, as evidenced by the data presented in Fig. 8A, which confirms the reusability of the prepared biosensor is excellent (In14 days, RSD 0.40%) for AD monitoring.
The stability study of the biosensor is crucial for reliable sensing devices. The stability of the prepared La/CF/rGO/ITO bioelectrode is demonstrated by utilizing the Rct value for up to 1–70 days, by a regular interval of five days at OEP. As a result of the stability investigation, it was concluded that the % RSD ranged from 0 to 9.9% for 1 to 70 days, as presented in Fig. 8B. After 70 days, the % RSD is more than 10%, which confirmed that the fabricated bioelectrode La/CF/rGO/ITO is stable because the CF and rGO on the electrode surface provides a solid electrostatic interaction for metal ions with oxygen-containing rGO in the electrolytic solutions. It has been found that the bioconjugated electrode is stable for up to 70 days in 80 μM (50 μl) AD solution at OEP. Thus, the EIS-based biosensor demonstrated good reusability and stability of the fabricated La/CF/rGO/ITO bioelectrode for monitoring AD neurotransmitters.
All the EIS studies were performed at pH 6.5 to detect AD. Fig. 8C shows a selectivity study of the fabricated biosensor towards AD by using the EIS technique in the presence of potential interfering analytes uric acid, dopamine, glutamic acid, urea, ascorbic acid, glucose, and lactic acid. The standard solution used in the selectivity test is 80 μM of each and 50 μl volume to investigate the analysis using the OEP. The biosensor response showed a % RSD change from 1.25 to 5.8% in the presence of these interfering analytes. These results signify the nanofabricated La/CF/rGO/ITO bioelectrode is highly selective, stable, reproducible, and practically viable for real sample monitoring of AD neurotransmitters. Thus, the CF/rGO nh is a reliable platform for detecting AD in the presence of various interfering analytes.
Under the same reaction conditions, EIS techniques were used to investigate the spiked BSA real sample with the standard AD analytes. Six distinct AD concentrations, namely 5, 10, 20, 40, 60, and 80 μM, were tested for spike-specified concentrations of AD in a fetal BSA solution in phosphate buffer at pH 6.5 in OEP. Fig. 8D displays the Rct response in the standard and BSA serum samples. Furthermore, Table 1 shows that standard and real BSA spike samples recovered at greater than the spiked concentrations and RSD below 8.3%. As a result, the EIS-based responses of the standard AD sample and the serum sample (spike BSA real samples) correspond well, and the CF/rGO nh was determined to be a superior material for AD biosensors in an enzymatic environment. Thus, the prepared biosensor is reliable for the selective monitoring of AD in real samples and important for neurodegenerative disorders.
Standard AD concentration added (μM) in BSA | Concentration determined in real BSA samples (μM) | Recovery (%) | RSD (%) |
---|---|---|---|
5 | 5.2 | 104 | 4 |
10 | 10.3 | 103 | 3 |
20 | 20.51 | 102.5 | 2.5 |
40 | 40.27 | 100.6 | 0.6 |
60 | 60.3 | 100.5 | 0.5 |
80 | 86.7 | 108.3 | 8.3 |
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4ma01216j |
‡ These authors contributed equally. |
This journal is © The Royal Society of Chemistry 2025 |