Open Access Article
Jiaxin
Zhang
a,
Valeria
Perez
a,
ThomasJae
Garcia
b,
Dan-il
Yoon
a,
David
Wagner‡
a,
Yanika
Schneider
a,
Min Hwan
Lee
b,
Sang-Joon John
Lee
*c and
Dahyun
Oh
*a
aDepartment of Chemical and Materials Engineering, San Jose State University, San Jose, California, USA. E-mail: dahyun.oh@sjsu.edu
bDepartment of Mechanical Engineering, University of California, Merced, Merced, California, USA
cDepartment of Mechanical Engineering, San Jose State University, San Jose, California, USA. E-mail: sang-joon.lee@sjsu.edu
First published on 3rd October 2024
Polyethylene oxide (PEO)-based solid composite electrolytes (SCEs), with inorganic fillers, are studied extensively due to their effective balance between mechanical and electrochemical properties. The correlation between the composition of SCEs and their electrochemical behavior has been studied extensively, primarily focusing on the type of polymer matrix with a bias towards high lithium (Li) salt. In this study, we examine the changes in the properties of SCEs at two low EO
:
Li ratios, 43
:
1 and 18
:
1, in the PEO-LiTFSI matrix (with and without 10 wt% of 5 μm LLZTO) and evaluate their impact on Li stripping and plating reactions. Although higher salt concentration (18
:
1) results in substantially higher ionic conductivity (by approximately an order of magnitude), interestingly we observe that lower salt concentration (43
:
1) exhibits up to 3 times longer Li cycling life. Notably, electrolytes with low salt concentration (43
:
1) are much stiffer, with compressive modulus more than twice as high as the 18
:
1 counterpart. Although the ionic conductivity of the electrolyte is often the most immediate concern in the electrolyte design process, these findings accentuate the equal importance of mechanical properties in order to ensure successful electrolyte performance throughout prolonged Li cycling.
PEO is often selected as a polymer substrate for electrolytes because of its excellent solubility with various salts, including lithium salts, allowing it to incorporate Li ions into its polymer matrix efficiently.14 However, PEO exhibits low ionic conductivity due to its crystallization below 60 °C.15 Reducing the crystallinity of PEO is a common design objective to enhance ion conduction, but low crystallinity may compromise mechanical strength. Adding an air-stable ion conductor such as LLZO or LLZTO (Li7La3Zr2Ta0.6O12) into the PEO-Li salt matrix has demonstrated improvements, not only in enhancing mechanical strength but also in enhancing ionic conductivities, especially for high EO
:
Li ratio (12
:
1 or 8
:
1) matrices.16,17 While existing studies on SCEs predominantly examine the effect of particle size, amount of particle loading, and particle surface treatment,16–19 it is crucial to recognize that the lithium salt concentration in PEO is another important design consideration. Lowering the necessary amount of lithium salt is desirable from a practical perspective because of its high cost. Prior research in PEO-LiTFSI (lithium bis(trifluoromethanesulfonyl)imide) electrolytes has explored the effect of varying lithium salt concentrations on ionic conductivity and crystallinity, where an increase in salt concentration resulted in a decrease in the degree of crystallinity.20,21 However, an important gap exists in our understanding of how concentrations of lithium salt change the mechanical properties of PEO-based composites electrolytes and the corresponding impact on the electrochemical reactions of Li.
In this work, we aim to bridge this gap by experimentally investigating PEO-based electrolytes at two low concentrations of lithium salt (LiTFSI, 18
:
1 (r = 0.055) vs. 43
:
1 (r = 0.023), (r = Li/EO22)) with and without 10 wt% 5 μm LLZTO. We study their chemical and thermal properties using Fourier-transform infrared spectroscopy (FTIR) and differential scanning calorimetry (DSC) and also examine their behavior under macroscopic compression as well as nanoscale surface adhesion measurements by atomic force microscopy (AFM). We also determine the effect of salt concentration and LLZTO on the Li stripping and plating reaction by testing in a Li half-cell, to make a direct correlation between the compressive modulus of SCEs and electrochemical reaction with Li. The mechanical behavior of SCEs under compression holds importance in the development of high-performance solid electrolytes, especially with respect to dendrite suppression.23 This work seeks to provide insights into both ionic transport and mechanical behavior, ultimately facilitating the design of advanced solid electrolytes tailored for practical applications.
:
1 (EO
:
Li molar ratio) without LLZTO, 18
:
1 with 10 wt% LLZTO, 43
:
1 without LLZTO, and 43
:
1 with 10 wt% LLZTO (subsequently abbreviated as 18
:
1 no LLZTO, 18
:
1 10% LLZTO, 43
:
1 no LLZTO, and 43
:
1 10% LLZTO, respectively). The PEO-LiTFSI electrolytes were fabricated using the solvent casting method. Before the fabrication, PEO (Mv = 600
000 g mol−1, Sigma-Aldrich), LiTFSI (Gotion, Inc.), and LLZTO (5 μm, Ampcera Inc.) were dried in a vacuum oven (PEO: at 40 °C for 48 h and LiTFSI/LLZTO: at 60 °C for 24 h). Anhydrous acetonitrile (ACN, Fisher Scientific, 99.8 + %) was dried for a week using molecular sieves (3 Å, baked at 350 °C for 3 hours). All electrolyte solutions used ACN as the solvent, with a weight ratio of 9
:
1 for a solvent to all solid components, including LiTFSI, PEO, and, where applicable, LLZTO. The mixtures were prepared by dissolving LiTFSI in ACN first, followed by the gradual addition of PEO and then stirred for 24 h. For samples including LLZTO, a 3 wt% of pre-dispersed LLZTO solution in ACN was added to the LiTFSI-PEO mixture and stirred for 24 h. The mixing was done inside a glovebox (MBraun Labstar, UHP Ar) and the mixture was cast onto a PTFE block using a doctor blade under N2. The drying process involved N2 flow at room temperature for 30 minutes, followed by vacuum drying at 65 °C for 30 minutes. The thickness of the cast electrolytes after drying ranged from 45 to 60 μm, and the films were stored in an Ar-filled glovebox and tested within one week after casting.
Galvanostatic cycling tests were conducted with symmetric cells (Li/Electrolyte/Li) at a constant current (0.2 mA cm−2) at 50 °C. The diameters of the Li disks and the electrolyte were 5 mm and 9.5 mm respectively. The electrolyte was nominally 50 μm thick, and the lithium disks were 0.75 mm thick. Linear sweep voltammetry (LSV) was performed in Li/Electrolyte/Cu cells from open circuit voltage (OCV) to 6.0 V at a scan rate of 0.1 mV s−1, for which the copper foil (MTI Corp.) was 9 μm thick. The symmetric and LSV cells were assembled inside an Ar-filled glove box using a custom-designed quartz cell (Fig. S1A, ESI†), modified from a gas-tight cell in the literature.24 After assembly, the symmetric cells were baked at 60 °C for 18
:
1 and at 65 °C for 43
:
1 for one hour. The baking temperatures were determined by the melting point using DSC.
:
1 and 10 s for 43
:
1) followed by vacuum-drying at 45 °C for 30 min. Each contact cycle (approach + retraction) was performed over ∼6 s with a maximum contact force of ∼200 nN. All nanomechanical probing was conducted in an environment chamber (∼1720 cm3) under dry nitrogen flow.
:
1 and 43
:
1) was studied using FTIR (Fig. 1A). The triplet peaks (1143 cm−1 to 1060 cm−1) associated with C–O–C stretching shared similar shapes with pure PEO in all samples, indicating that the Li concentration used in this study is relatively low.27 The peaks corresponding to –CH2 at 1466, 962, and 841 cm−1,16,27 decreased as the salt concentration increased. These peaks were normalized against the one near 1109 cm−1 to compare their relative intensities, showing 25–42% reduced intensity of the high salt electrolyte (18
:
1) compared to the low salt electrolyte (43
:
1) (Table S1, ESI†). The normalized peak intensity at 1190 cm−1 corresponding to the CF3 stretching mode of TFSI28 increased with the high salt electrolyte, indicating the complexation of PEO with TFSI− (Table S1, ESI†).27 The peaks at 739 cm−1 which originate from the CF3 symmetric deformation of the free anion, are heightened (66–100% from low to high salt electrolyte) as salt concentrations increase,29 (Table S1, ESI†), suggesting a higher concentration of free Li ions. However, there were no significant changes in FTIR spectra when LLZTO was introduced, indicating that LLZTO does not alter LiTFSI dissociation. Doublet peaks (1360 cm−1 to 1340 cm−1), attributed to CH2 asymmetric bonding, were also evident across all compositions, indicating the presence of crystalline PEO in all four solid-state electrolytes used in this study.30 Among these doublet peaks, electrolytes with lower salt concentrations exhibited more intense peaks at 1340 cm−1 than those with higher salt concentrations, consistent with prior findings in PEO systems.27,31
![]() | ||
Fig. 1 (A) FTIR spectra, (B) DSC thermograms, (C) and (D) crystallinity and melting temperature plots (averaged values of two replicates) of electrolytes with varied EO : Li ratios and LLZTO content. | ||
The effects of LiTFSI salt concentration and inorganic fillers on the thermal behavior and the degree of crystallinity of PEO-LiTFSI electrolytes were studied using DSC (Fig. 1B, Table S2, ESI†). All of the electrolytes exhibited endothermic peaks within the temperature range of 52 °C (18
:
1) to 63 °C (43
:
1) due to the melting of PEO. Electrolytes containing higher salt concentrations (18
:
1) displayed lower melting temperatures, owing to the plasticizing effect of LiTFSI.21 Meanwhile, the introduction of LLZTO had minimal influence on the melting temperature of the electrolytes. Fig. 1C shows the average degree of crystallinity for the different electrolytes. Overall, the crystallinity of electrolytes with lower salt concentrations (43
:
1) was higher than the high salt counterpart (18
:
1). It is generally accepted that the inorganic fillers reduce the crystallinity of PEO;32,33 however, we observed that the inorganic fillers influence the overall crystallinity of PEO-LiTFSI electrolytes differently, depending on the salt concentrations. Adding 10 wt% of LLZTO to electrolytes with lower salt concentrations (43
:
1) led to an increase in the crystallinity, with values rising from 49% to 58%. In comparison, the impact of LLZTO on crystallinity was not evident for the higher salt concentrations (32% without, 33% with LLZTO).
While DSC revealed bulk crystallinity values, optical images were taken to examine morphological differences. In the 18
:
1 electrolyte (representative images shown in Fig. 2A and B), the spherulite boundaries exhibited more distinct contrast than in the 43
:
1 case (representative images shown in Fig. 2C and D). The corresponding binarized images are shown at the upper right inset for each case, with the interior regions of spherulites shown in black pixels and amorphous regions shown in white pixels. The 18
:
1 electrolytes exhibit less densely packed spherulites (i.e., lower crystalline area fraction) than the 43
:
1 case. Comparing images of no-LLZTO images, the area fraction of spherulites (i.e., proportion of crystalline regions) was 87% ± 4.6% (average ± standard deviation sampling n = 4 replicates for each case) for the 18
:
1 electrolytes and 93% ± 1.2% for the 43
:
1 electrolytes. The corresponding images with LLZTO particles (Fig. 2B and D) are qualitatively similar for the different salt concentrations but are not evaluated quantitatively because the particles are nonuniformly superimposed upon both crystalline and amorphous regions (along the z-axis, perpendicular to the image plane). Although limited to a 2-D imaging plane in Fig. 2, the observed larger area fraction for 43
:
1 is consistent with DSC results (Fig. 1D) that also revealed larger volumetric crystallinity for the 43
:
1 case.
The mechanical response of the four types of electrolytes under compression was studied to understand potential implications for future use in fully assembled batteries that have confined volume (Fig. 3A). It was observed that the 18
:
1 electrolyte without LLZTO exhibited a lower compressive modulus at 0.9 kPa (computed as a linear-equivalent for strain energy density up to 50% strain) compared to the 43
:
1 electrolyte, which had a compressive modulus of 14.6 kPa. This difference in mechanical properties can be attributed to the higher proportion of amorphous regions in the 18
:
1 series, rendering them more susceptible to deformation.34 Although both 18
:
1 electrolytes with and without LLZTO exhibited similar crystallinity, the introduction of LLZTO led to increased stiffness (9.5 times for 18
:
1 and 32% for 43
:
1) in the CPE. Among the tested electrolytes, the 43
:
1 10 wt% LLZTO composition exhibited the highest compressive modulus of 19.3 kPa, owing to its highly ordered arrangement of polymer chains and the presence of LLZTO. In contrast, the 18
:
1 10 wt% LLZTO CPE had a lower compressive modulus of 8.6 kPa.
Nanoscale indentation measurements with an AFM probe were performed to quantify differences in surface adhesion. As shown in Fig. 3B, the adhesion force between the AFM probe and sample was 49.2 ± 4.5 nN and 35.5 ± 6.9 nN (mean ± standard deviation, n = 50) for EO
:
Li ratios of 18
:
1 and 43
:
1, respectively. Differences appeared in measured values based on measurement location, while less variation was detected between cycles at a specific location. The observed behavior is consistent with macroscopic stress–strain behavior, in that the higher adhesion energy for the 18
:
1 case corresponds to greater compliance and, thus, higher conformality of the polymer with the indenting probe. Samples containing LLZTO were not tested with AFM due to its high surface roughness and spatial nonuniformity near and far from LLZTO particles.
Electrochemical evaluations were conducted to understand the interplay of the structural, mechanical, and surface properties in the electrochemical performance of solid electrolytes. The average ionic conductivities of 18
:
1 no LLZTO, 18
:
1 10% LLZTO, 43
:
1 no LLZTO, and 43
:
1 10% LLZTO were 6.08 × 10−6, 1.98 × 10−6 1.83 × 10−7, and 1.51 × 10−7 S cm−1, respectively, at room temperature. Fig. 4A shows that a higher Li salt concentration (18
:
1) increases ionic conductivity. However, large variability was observed in the higher Li salt concentration (18
:
1), which suggests poor homogeneity of the high-salt electrolytes. Furthermore, the addition of 10% LLZTO showed no beneficial effect on the ionic conductivity of both the high and low salt systems. There was a 67% reduction in ionic conductivity for 18
:
1, while a 17% reduction in ionic conductivity for 43
:
1 after adding LLZTO. We believe that the ion conduction might be partially interrupted due to the presence of LLZTO particles35 to a greater extent for the high salt electrolyte, even though their crystallinity remains similar with and without LLZTO (based on DSC results). The decrease of ionic conductivity34 or the increase/minimal impact on the PEO crystallinity30 by adding the inorganic fillers were reported in other related studies for low salt containing electrolytes (less than 16
:
1 of EO
:
Li). The electrochemical stability windows of four electrolytes were determined using LSV measurement at room temperature (Fig. 4B). The threshold voltages are selected as the voltage at which an abrupt increase in current (e.g., 3 × 10−7 A) is observed,36 The corresponding values were 4.87 V, 4.79 V, 4.89 V, and 5.03 V for 18
:
1 no LLZTO, 18
:
1 10% LLZTO, 43
:
1 no LLZTO, and 43
:
1 10% LLZTO, respectively. Oxidation occurred within the range of 4.70 to 4.95 V due to the decomposition of the material. Furthermore, a reduced oxidation current was observed in the low-salt electrolytes compared to the high-salt electrolytes.
Galvanostatic cycling using half-cell tests were conducted to study the long-term effects of electrolyte properties on the Li stripping and plating behavior. Representative data for each electrolyte composition was selected from 4 to 5 replicates. We observed a sudden, significant voltage drop and fluctuating voltage profiles for both low and high modulus electrolytes when a short circuit occurred. Among the four compositions, the 43
:
1 ratio of 10% LLZTO exhibited the most stable performance up to 350 cycles, 2 to 3 times higher cycle numbers than other compositions (Fig. 4C–F). This is an interesting result because the 43
:
1 10% LLZTO electrolyte exhibited the highest compressive modulus and the lowest ionic conductivity than other compositions and the surface adhesion of the 43
:
1 electrolyte was lower than that of the 18
:
1 case. While the high salt electrolytes had higher ionic conductivities, lower crystallinity, and better surface adhesion (leading to better electrode contact), their cycling performance was poor. Solid-state electrolytes with high mechanical strength are known to be better at suppressing lithium dendrites, preventing their penetration into polymers during prolonged Li cycling.16,17 Our findings not only accentuate the importance of mechanical properties for achieving superior Li cycling for an extended period of time, but also show the direct trade-off with respect to ionic conductivity.
:
1 vs. 43
:
1) and the use of micron-size inorganic ceramic fillers, LLZTO. We examined the chemical bonding, morphological, mechanical, and electrochemical characteristics of solid-state electrolytes. We observed the beneficial effects of higher salt concentrations compared to lower salt concentration on ionic conductivity and surface adhesion, demonstrating a remarkable increase in ionic conductivity for 18
:
1 over 43
:
1, ranging from 13 (with LLZTO) to 33 times (without LLZTO). Additionally, there was a notable (38%) enhancement in surface adhesion at higher salt concentration. However, lower salt concentrations (43
:
1), especially in combination with LLZTO, displayed 2 to 3 times longer Li cycling life, attributed to increased crystallinity (35–43% higher than 18
:
1) and higher resistance to deformation (55% higher compressive modulus than 18
:
1) during Li cycling. In addition to its advantageous bulk properties, including a high modulus, we expect that the interfacial stability of this low-salt solid-state electrolyte can be improved by adding compounds like fluoroethylene carbonate37,38 or lithium nitrate,39,40 thereby enhancing lithium cycling performance. These reported trade-offs between high ionic conductivity and long-duration Li cycling emphasize the importance of salt concentration and filler particles on the optimization of material design for solid-state polymer electrolytes.
Footnotes |
| † Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4ya00467a |
| ‡ Present address: Department of Chemical Engineering, The University of Utah. |
| This journal is © The Royal Society of Chemistry 2024 |